NAVY MIL-DTL-32149 A-2007 CLOTH WATERPROOF FLAME RESISTANT MOISTURE VAPOR PERMEABLE《防水阻燃利于水分渗透衣》.pdf
《NAVY MIL-DTL-32149 A-2007 CLOTH WATERPROOF FLAME RESISTANT MOISTURE VAPOR PERMEABLE《防水阻燃利于水分渗透衣》.pdf》由会员分享,可在线阅读,更多相关《NAVY MIL-DTL-32149 A-2007 CLOTH WATERPROOF FLAME RESISTANT MOISTURE VAPOR PERMEABLE《防水阻燃利于水分渗透衣》.pdf(20页珍藏版)》请在麦多课文档分享上搜索。
1、NOT MEASUREMENTSENSITIVE MIL-DTL-32149A 30 January 2007 SUPERSEDING MIL-DTL-32149 28 April 2004 DETAIL SPECIFICATION CLOTH, WATERPROOF, FLAME RESISTANT, MOISTURE VAPOR PERMEABLE This specification is approved for use by all Departments and Agencies of the Department of Defense. 1. SCOPE 1. Scope. Th
2、is document covers flame resistant, waterproof, and moisture vapor permeable cloth used in the ruggedized flyers coveralls. 2. APPLICABLE DOCUMENTS 2.1 General. The documents listed in this section are specified in sections 3 and 4 of this specification. This section does not include documents cited
3、 in other sections of this specification or recommended for additional information or as examples. While every effort has been made to ensure the completeness of this list, document users are cautioned that they must meet all specified requirements of documents cited in sections 3 and 4 of this spec
4、ification, whether or not they are listed. 2.2 Government documents. 2.2.1 Specifications. The following specification forms a part of this document to the extent specified herein. Unless otherwise specified, the issue of this document is that cited in the solicitation or contract. Comments, suggest
5、ions, or questions on this document should be addressed to: Commander, Naval Air Warfare Center Aircraft Division (Code 491000B120-3), Highway 547, Lakehurst, NJ 08733-5100 or emailed to thomas.omaranavy.mil. Since contact information can change, you may want to verify the currency of this address i
6、nformation using the ASSIST Online database at http:/assist.daps.dla.mil. AMSC N/A FSC 8305 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-MIL-DTL-32149A DEPARTMENT OF DEFENSE SPECIFICATION MIL-DTL-83133 - Turbine Fuels, Aviation, Kerosene Types, NA
7、TO F-34 (JP-8), NATO F-35, and JP-8+100 (Copies of this document are available online at http:/assist.daps.dla.mil/quicksearch/ or http:/assist.daps.dla.mil or from the Standardization Document Order Desk, 700 Robbins Avenue, Building 4D, Philadelphia, PA 19111-5094.) 2.2.2 Other Government document
8、s and drawings. The following other Government documents and drawing form a part of this document to the extent specified herein. Unless otherwise specified, the issues of these documents are those cited in the solicitation or contract. CODE OF FEDERAL REGULATION 27 CFR 21 - Formulas for Denatured A
9、lcohol and Rum (Copies of this document are available online at www.gpoaccess.gov/cfr/about.html or from the Superintendent of Documents, U.S. Government Printing Office, North Capital WVP in g(Pa*m2*h) WVPapp = water vapor permeability apparatus4.4.7 Colorfastness. 4.4.7.1 Laundering. Laundering sh
10、all be tested as specified in AATCC Test Method 61, Test 1A, 3 cycles. 1993 AATCC Standard Reference Detergent WOB (without fluorescent whitening agent and without phosphate) shall be used. 4.4.8 Synthetic perspiration test. The specimen, 8 by 8 inches, shall be cut and exposed to synthetic perspira
11、tion as follows: The synthetic perspiration solution shall be made by combining 3.0 grams sodium chloride, 1.0 gram trypticase soy broth powder, 1.0 gram normal propyl propionate, 0.5 gram of liquid lecithin and 500 ml of distilled water. Cover the solution and heat to 50 C, stirring frequently whil
12、e heating. Continue until all ingredients are dissolved. Then, cool the solution to 35 C, remove cover and dispense it immediately with a pipette or other measuring device. Dispense 2 ml of perspiration solution at 35 C onto the center of an 8- by 8- by 1/4 inch glass plate. Place the specimen on th
13、e glass plate with the back side contacting the glass. Dispense an additional 2 ml of the synthetic perspiration solution onto the center of the 15 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-MIL-DTL-32149A specimen. Place a second 8- by 8- by 1/
14、4-inch glass plate on top of the specimen and then place a 4 pound weight on top of the assembly in the center. After 16 hours, remove the specimen (do not rinse) and air dry the specimen before testing as specified in AATCC Test Method 15. 4.4.9 Contamination procedure. The specimen (or specimen ar
15、ea) shall be laid flat, face side up, on a glass plate. Three drops (1ml for sealed samples) of a test liquid, either hydraulic fluid or JP-8 conforming to MIL-DTL-83133, shall be applied to the center of the specimen (or specimen area). A glass plate of the same dimensions shall be placed on the sp
16、ecimen (or specimen area) and a pressure of 0.0625 pounds per square inch (1 pound per square inch for seam sealed samples) of glass plate contact area shall be applied to the assembly. After 16 hours (2 hours for seam sealed samples), remove the specimen (or specimen area) from the assembly and tes
17、t immediately for the required performance property in the center of specimen (or specimen area). For testing the initial condition, the test specimen shall be as specified by the applicable test method. For testing hydrostatic resistance and leakage after laundering, one laundering sample 48 inches
18、 by the full width of the cloth shall be used for each test liquid specified above. Three drops of the test liquid shall be applied to each laundering sample. The face side of the laundering sample shall be marked using a laundry marker pen. The laundering test shall then be conducted in accordance
19、with 4.4.10 for one laundering and drying cycle. After laundering, the specimen areas may be cut from the laundering sample to facilitate performance property testing. Ten specimens shall be tested for each of the initial and the after laundering conditions. 4.4.9.1 Contamination procedure after air
20、craft fluids. The specimen (or specimen area) shall be laid flat, face side up, on a glass plate. One milliliter of JP-8 fuel conforming to MIL-DTL-83133 shall be spread over the middle of the sample, followed by 1 ml of de-icing fluid conforming to SAE-AMS1424. The samples shall then be placed flat
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- NAVYMILDTL32149A2007CLOTHWATERPROOFFLAMERESISTANTMOISTUREVAPORPERMEABLE 防水 阻燃 利于 水分 渗透 PDF

链接地址:http://www.mydoc123.com/p-978804.html