FORD WSS-M4G320-A4-1997 SEALER SILICONE RUBBER OXIME CURED LOW VISCOSITY《低粘度肟固化硅橡胶密封剂》.pdf
《FORD WSS-M4G320-A4-1997 SEALER SILICONE RUBBER OXIME CURED LOW VISCOSITY《低粘度肟固化硅橡胶密封剂》.pdf》由会员分享,可在线阅读,更多相关《FORD WSS-M4G320-A4-1997 SEALER SILICONE RUBBER OXIME CURED LOW VISCOSITY《低粘度肟固化硅橡胶密封剂》.pdf(5页珍藏版)》请在麦多课文档分享上搜索。
1、 ENGINEERING MATERIAL SPECIFICATIONMaterial Name Specification NumberDate Action Changes1997 10 13 Revised Revised para 3.7; Updated N. Vallabhanath1996 08 12 Activated N. VallabhanathWP 3948-a Page 1 of 5SEALER, SILICONE RUBBER, OXIME CURED, WSS-M4G320-A4LOW VISCOSITY1. SCOPEThe material defined by
2、 this specification is a one component thixo-tropic spreadable oxime based silicone rubber adhesive/sealant with goodheat and oil resistance. It cures progressively inward from the surfaceat room temperature absorbing water vapor in the air as the curingactivator.2. APPLICATIONThis specification was
3、 released originally for material used for wipermotor application.3. REQUIREMENTS3.1 QUALITY SYSTEM REQUIREMENTSMaterial suppliers and part producers must conform to QualitySystem Requirements, QS-9000. Material specification requirementsare to be used for initial qualification of materials. A Contr
4、olPlan for ongoing production verification is required. This planmust be reviewed and approved by the relevant Ford Materialsactivity and/or Ford Supplier Technical Assistance (STA) prior toproduction parts submission. Appropriate statistical tools must beused to analyze process/product data and ass
5、ure consistentprocessing of the materials.Part producers using this material in their products, must use Fordapproved materials and must conform to a process control plan whichhas been approved by STA and/or the relevant Materials Activity.3.2 INFRARED SPECTROPHOTOMETRY AND/OR THERMAL ANALYSISFord M
6、otor Company, at its option, may conduct infrared and/orthermal analysis of material/parts supplied to this specification.The IR spectra and thermograms established for initial approvalshall constitute the reference standard and shall be kept on fileat the designated material laboratory. All samples
7、 shall produce IRspectra and thermograms that correspond to the reference standardwhen tested under the same conditions.ENGINEERING MATERIAL SPECIFICATION WSS-M 4G320-A4WP 3948-b Page 2 of 53.3 CONDITION ING AND TEST CONDITIONSAll test values indicated herein are based on material conditionedin a co
8、ntrolled atmosphere of 23 +/- 2 C and 50 +/- 5 % relativehumidity for not less than 24 h prior to testing and tested underthe same conditions unless otherwise specified.3.4 SPECIFIC GRAVITY 1.27 - 1.35(ASTM D 1475)3.5 VISCOSITY, range 100 - 300 g/(FLTM BV 103-01, extrusion rate at 620 kPa minuteair
9、pressure and 3.2 mm diameter orifice)3.6 FLOW CHARACTERISTICS 7.5 mm max(ASTM D 2202 after 3 minutes)3.7 CURE RATE - TACK FREE TIME 10 - 15 minutesA 6 mm diameter x 150 mm long bead shall be tack free in 15 minutesmax and completely cured in 168 h max, at 23 +/- 2 C and 50 +/- 5 %relative humidity.A
10、 tack free skin will form in 15 minutes. The bead must be testedas applied. Cure time is affected by relative humidity, degree ofconfinement, and cross-sectional thickness.Generally, a 6 mm bead will cure within 24 h at 23 +/- 2 C and 50+/- 5 % RH. The time for proper cure is generally lengthened by
11、increased confinement.3.8 LOW TEMPERATURE FLEXIBILITY No crackingTest Method: Apply a 3 mm diameter x 150 mm long bead of materialto a strip of aluminum foil. Cure for 48 h at 23 +/- 2 C and 50 +/-5 % RH. Expose to a temperature of - 40 +/- 2 C for 4 h and bendaround a temperature conditioned 3.2 mm
12、 mandrel.3.9 HIGH TEMPERATURE RESISTANCETest Method: Condition ASTM test sheets for 7 d at 23 +/- 2 C and50 +/- 5 % RH. Heat in an air circulating oven and hold for 168 hat 175 +/- 2 C. Cool to room temperature and test.3.9.1 Tensile Strength, min 1.7 MPa(ASTM D 412, Die C)3.9.2 Elongation, min 300
13、%(ASTM D 412, Die C)3.10 FLUID IMMERSION RESISTANCE(24 h at 38 +/- 2 C in windshield washersolution WSE-M8B16-B)3.10.1 Tensile Strength, min 1.4 MPa(ASTM D 412, Die C)ENGINEERING MATERIAL SPECIFICATION WSS-M 4G320-A4WP 3948-b Page 3 of 53.10.2 Elongation, min 350 %(ASTM D 412, Die C)3.10.3 Hardness
14、Shore A, range 28 - 63(ASTM D 2240, 15 s dwell, ply upspecimens to 6 m m total thickness)3.10.4 Weight Change, max 5 %Test Method: Apply material 0.5 mm thick approximately 50mm long to weighed clean 25 x 100 mm aluminum or stainlesssteel panels. Cure for 48 h at standard conditions. Weighto determi
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- FORDWSSM4G320A41997SEALERSILICONERUBBEROXIMECUREDLOWVISCOSITY 粘度 固化 硅橡胶 密封剂 PDF

链接地址:http://www.mydoc123.com/p-753793.html