1、Designation: F 1782 97 (Reapproved 2002)Standard Practice forAmount of Ink Deposit on Fabric Type Ribbons1This standard is issued under the fixed designation F 1782; the number immediately following the designation indicates the year oforiginal adoption or, in the case of revision, the year of last
2、revision. A number in parentheses indicates the year of last reapproval. Asuperscript epsilon (e) indicates an editorial change since the last revision or reapproval.1. Scope1.1 This practice covers the determination of the amount ofink deposit, sometimes known as ink content, on inked fabricribbons
3、.1.2 This standard does not purport to address all of thesafety concerns, if any, associated with its use. It is theresponsibility of the user of this standard to establish appro-priate safety and health practices and determine the applica-bility of regulatory limitations prior to use. See 6.1 and 9
4、.4 forspecific precautionary statements.2. Referenced Documents2.1 ASTM Standards:D 685 Practice for Conditioning Paper and Paper Productsfor Testing2F 221 Terminology Relating to Carbon Paper and InkedRibbon Products and Images Made Therefrom23. Terminology3.1 For definitions of terms used in this
5、test method, refer toTerminology F 221.4. Summary of Practice4.1 The amount of ink deposit is gravimetrically determinedby analytically weighing a conditioned test specimen. The inkdeposit is removed by the use of a suitable solvent(s) in anultrasonic cleaner. The de-inked fabric sample is condition
6、edand reweighed. The amount of ink deposit is calculated.5. Apparatus5.1 Analytical Balance, with a sensitivity to 0.1 mg.5.2 Ultrasonic Bath, with or without heater.6. Reagents6.1 Care should be taken to select the extraction solvent(s)so that only the ink is removed from substrates. WarningVapors
7、from solvents can be toxic when inhaled over pro-longed periods. Some solvents commonly used may be listedas carcinogenic. Others are flammable and suitable precautionsshould be taken. Handle with care and use only in properlyventilated areas to avoid breathing vapors. A fume hood isrecommended.7. C
8、onditioning7.1 Allow the test specimen to stabilize under room condi-tions for 15 min for routine testing.7.2 Allow the test specimen to condition1hat23.06 2.0Cand 50 6 2 % relative humidity for a more precise determina-tion (see Practice D 685).8. Test Specimen8.1 Cut a representative test sample o
9、f the desired size fromthe conditioned specimen.9. Procedure9.1 From a sample that has been conditioned in accordancewith 7.1 or 7.2, discard at least two outer wraps of ribbonmaterial if from a reel of inked fabric prior to sampling. If thesample to be checked is from a ribbon cartridge, pull out s
10、omeof the ribbon in order to check the ink inside the cartridge.9.2 For a narrow fabric ribbon sample, typically 1 in. or lessin width, cut a 10 to 15 in. long section for ink percentagecalculation. For wide fabric ribbons, typically 14 in. or greaterin width, cuta2by3in.portion from the right and l
11、eft sidesfor ink percentage calculation. This helps to determine if thefabric is inked evenly across the width of the fabric. For gramsper square metre calculation, a popular scaling factor for thesample is1200 of a square metre for ribbons12 in. (12.7 mm)or less and1100 of a square metre for ribbon
12、s above12 in. (12.7mm). Care should be taken to avoid contact of sample with inkabsorbing surfaces. (Example: Cardboard, paper towel, etc.)Sheet mylar or similar surfaces are acceptable.9.3 Weigh the sample in accordance with acceptable ana-lytical procedure. Weigh to the nearest 0.1 mg. Record as i
13、nkedweight (A).9.4 Set up the ultrasonic bath by first filling the tank with atransfer medium (for example, warm tap water plus a wettingagent/detergent). Place two glass beakers (400 or 600 mL) ofthe desired solvent(s) in a beaker positioning cover to suspendthe beakers in the bath. Plug in the ult
14、rasonic bath and turnpower on. If using a bath with a heater, turn the heat switch toon and allow the bath to stabilize to the desired temperature.WarningThe temperature of the bath should not exceed theboiling point of the solvent.1This practice is under the jurisdiction of ASTM Committee F05 on Bu
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
5000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- ASTMF178219972002STANDARDPRACTICEFORAMOUNTOFINKDEPOSITONFABRICTYPERIBBONS 帘布 轮胎 带状 结构 油墨 沉积 标准 操作规程 PDF

链接地址:http://www.mydoc123.com/p-535623.html