1、Designation: D4931 06 (Reapproved 2011)Standard Test Method forGross Moisture in Green Petroleum Coke1This standard is issued under the fixed designation D4931; the number immediately following the designation indicates the year oforiginal adoption or, in the case of revision, the year of last revis
2、ion. A number in parentheses indicates the year of last reapproval. Asuperscript epsilon () indicates an editorial change since the last revision or reapproval.1. Scope1.1 This test method covers both the preparation procedurefor samples containing free water (air drying loss (ADL) ongross moisture
3、samples) and the determination of the grossmoisture content of green petroleum coke.1.2 The values stated in SI units are to be regarded asstandard. The values given in parentheses are for informationonly.1.3 This standard does not purport to address all of thesafety concerns, if any, associated wit
4、h its use. It is theresponsibility of the user of this standard to establish appro-priate safety and health practices and determine the applica-bility of regulatory limitations prior to use.2. Referenced Documents2.1 ASTM Standards:2D2013 Practice for Preparing Coal Samples for AnalysisD2234/D2234M
5、Practice for Collection of a Gross Sampleof CoalD3302 Test Method for Total Moisture in CoalE11 Specification for Woven Wire Test Sieve Cloth and TestSieves3. Terminology3.1 Definitions of Terms Specific to This Standard:3.1.1 air drying, na process of partial drying of a greenpetroleum coke sample
6、to bring it to near equilibrium with theatmosphere in the room in which further reduction/division ofthe petroleum coke sample is to take place.3.1.2 air dry loss, ADL, nthe loss in mass, expressed as apercentage, resulting from each air drying operation.3.1.3 free water, nvisible unbound water in t
7、he sample.3.1.4 green petroleum coke, nsame as raw petroleumcoke.3.1.5 gross moisture, nthat moisture determined as theloss in mass in an air atmosphere under rigidly controlledconditions of temperature, time, and air flow.3.1.5.1 DiscussionTest Method D3302 prescribes theabove controlled conditions
8、.3.1.6 petroleum coke, nsolid, carbonaceous residue pro-duced by thermal decomposition of heavy petroleum fractions,or cracked stocks, or both.3.1.7 residual moisture, nthat moisture remaining in thesample after air drying.3.1.8 total moisture, nsynonym for gross moisture.4. Summary of Test Method4.
9、1 This test method is based on the loss in mass of a greenpetroleum coke sample in an air atmosphere under controlledconditions of temperature, time, and air flow.4.1.1 Preparation Procedure shall be used when the petro-leum coke sample contains free water. The gross moisturesample is weighed and ai
10、r dried to equilibrate it with theatmosphere. Determination of residual moisture is that deter-mined using the Drying Oven Method. Air drying and residualmoisture losses are combined to report gross moisture.4.1.2 Drying Oven Method shall be used in routine com-mercial practice when the sample does
11、not contain free water.The sample is crushed to at least minus 25 mm (1 in.) top sievesize and divided into analytical portions of at least 500 g each.Determination of total gross moisture is calculated by summingthe results of the Drying Oven Method and the results of thePreparation Procedure.5. Si
12、gnificance and Use5.1 Moisture adds weight to the coke and serves no usefulpurpose. A knowledge of the moisture content is important inthe purchase and sale of green petroleum coke, both of whichare conducted on a dry basis.5.2 The collection of the sample as specified for the DryingOven Method is i
13、ntended for the express purpose of determin-ing the total moisture of green petroleum coke. The standard is1This test method is under the jurisdiction of ASTM Committee D02 onPetroleum Products and Lubricants and is the direct responsibility of SubcommitteeD02.05 on Properties of Fuels, Petroleum Co
14、ke and Carbon Material.Current edition approved May 1, 2011. Published August 2011. Originallyapproved in 1989. Last previous edition approved in 2006 as D493106. DOI:10.1520/D4931-06R11.2For referenced ASTM standards, visit the ASTM website, www.astm.org, orcontact ASTM Customer Service at servicea
15、stm.org. For Annual Book of ASTMStandards volume information, refer to the standards Document Summary page onthe ASTM website.1Copyright ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.available to producers, sellers, and consumers for determin
16、a-tion when other techniques or modifications are not mutuallyagreed on.5.3 The Preparation Procedure is used only when samplecontains free water. Obtaining a representative sample of acoke source is compounded by the presence of free water.6. Apparatus6.1 Ovens:6.1.1 Air Drying OvenA device for pas
17、sing slightlyheated air over the sample. The oven shall be capable ofmaintaining a temperature of 10 to 15C (18 to 27F) aboveambient with a maximum oven temperature of 40C (104F)unless ambient temperature is above 40C (104F), in whichcase ambient temperature shall be used. Air changes are to beat th
18、e rate of 1 to 4/min. A typical oven is shown in Fig. 1.6.1.2 Drying Oven (for residual moisture on minus 25-mm(1.0-in.) samples sieve USAstandardforced-air type). It shallbe capable of maintaining a temperature of 105 6 5C and soconstructed that fresh air is introduced to all parts of the ovento en
19、sure the removal of moisture-laden air. Air flow shall bemaintained at sufficiently low velocity to prevent loss of fineparticles, (for example, one exchange per minute).6.2 Drying Pans:6.2.1 Pans for the gross moisture sample (PreparationProcedure) shall be noncorroding, weight-stable at temperatur
20、eused, and large enough so that the sample can be spread to adepth of not more than twice the diameter of the largestparticles, or not more than 25 mm (1.0 in.) depth for smallercoke. The pan sides shall be 50 to 75 mm (2 to 3 in.) high.6.2.2 Pans for crushed and divided sample shall be noncor-rodin
21、g, weight-stable at temperature used, and large enough sothat the sample can be spread to depth of not more than 50 mm(2 in.). The sides shall be not more than 75 mm (3 in.) high.6.3 Balances:6.3.1 Balance (Gross Sample)A balance with a minimumcapacity of 10 kg and sensitive to 1 g.6.3.2 Balance (Cr
22、ushed Sample)A balance with a mini-mum capacity of 4 or sufficient to weigh the pan, sample, andcontainer and sensitive to 0.1 g.6.4 Laboratory Sample ContainersNoncorroding canswith airtight, friction top or screw top sealed with a rubbergasket and pressure-sensitive tape for use in storage andtran
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- ASTMD493120062011STANDARDTESTMETHODFORGROSSMOISTUREINGREENPETROLEUMCOKE 出炉 石油 焦炭 含水量 标准 试验 方法 PDF

链接地址:http://www.mydoc123.com/p-518432.html