1、NAVISTAR, INC. TMS (TRUCK MATERIAL SPECIFICATION) NUMBER: TMS-6500 TITLE: Cellular Polyurethane, Integral Skin CURRENT REV No: 0810 DATE: October 2008 WRITTEN/EDITED BY: Materials Engineering APPROVED BY: Materials Engineering SUPERSEDES: Rev. A-1 - August 2001 PRINTED COPIES OF THIS DOCUMENT MUST B
2、E VERIFIED FOR CURRENT REVISION This specification may involve hazardous materials, equipment, and procedures. This specification does not purport to address all of the safety issues associated with its use. The user is responsible to consult appropriate safety and health practices and to determine
3、the applicability of regulatory limits prior to use. Change Notice: Replaced “International Truck and Engine Corporation” with “Navistar, Inc.” per corporate directive; added CEMS B-50 requirements; added insert adhesion requirements; modified Section 5; editorial changes. Reference: File 30-16B Key
4、words: Urethane Foam; Interior Trim 1.0 APPLICATION This specification covers a molded cellular polyurethane foam which forms an integral skin and is suitable for use in certain interior truck trim applications. 2.0 SCOPE This specification covers the general requirements, property and performance r
5、equirements, quality, quality control, and source approval for the coating, the integral skin, and the cellular polyurethane foam. 2.1 Restricted Chemical SubstancesEffective January 1, 2007, all product supplied to the requirements of this specification must comply with the requirements of the CEMS
6、 B-50 specification. 3.0 REFERENCE DOCUMENTS Unless otherwise specified, the latest issue of all referenced standards shall apply. The following standards, specifications and regulations are referenced in this specification. Quality System Standard ISO 9001 or TS-16949 ASTM D 3574 ASTM D 2247 NAVIST
7、AR Manufacturing Standard MS-D-13 ASTM D 624 ASTM D 412 CFR Title 29, Part 1910 ASTM D 2240 ASTM D 653 FMVSS 302 ASTM D 3359 ASTM D 47 NAVISTAR TMS-9544 ASTM D 3884 ASTM G 53 ASTM D 429 SAE J323 SAE J861 TMS-9543 4.0 GENERAL REQUIREMENTS 4.1 Color, Finish, and Texture This document is restricted and
8、 may not be sent outside Navistar, Inc. or reproduced without permission from Corporate Technical Standards. Suppliers are required to assume all patent liability. 2008 by Navistar, Inc. Color shall be specified on the engineering drawing for each part number. Color must match Navistar Paint Chip Co
9、lor Standards (available from Materials Engineering, TDTC). Color, finish, and texture of parts supplied to this specification must match the approved pre-production samples on file in the Industrial Design Department, TDTC. OCTOBER 2008 Page 1 of 5 NUMBER: TITLE: REVISION: TMS-6500 Cellular Polyure
10、thane, Integral Skin 0810 This document is restricted and may not be sent outside Navistar, Inc. or reproduced without permission from Corporate Technical Standards. Suppliers are required to assume all patent liability. 2008 by Navistar, Inc. OCTOBER 2008 Page 2 of 5 4.2 Coating Thickness, min: 0.2
11、5mm (0.01 inch) Color: To match Navistar color paint chip for the color specified on the engineering drawing. 4.3 Integral Skin Thickness: 6.4 1 mm (0.25 .04 inch) Pigmented to provide 90% color match to the color specified on the part drawing. 4.4 Cellular Polyurethane Elastomer Density, (ASTM D 35
12、74, Method A) Core Sample: 10 kg/m (0.62 lbs/ft) minimum Color: Pigmented to provide 90% color match to the color specified on the part drawing. 4.5 Property And Performance Requirements Material supplied shall meet all requirements of this specification unless otherwise specifically designated on t
13、he engineering drawing. 4.5.1 Finished Parts 4.5.1.1 Hardness ASTM D2240, Method A: Required: 50 5 points 4.5.1.2 Dry Heat Age - ASTM D 3574 Test K except as indicated below: Short term test - 1 hour at 100C (212F) Long term test - 168 hours at 65C (150F) Required: There shall be no blistering, soft
14、ening, or discoloration. Hardness shall not increase by more than 10 points. 4.5.1.3 Adhesion to Inserts ASTM D 429 Method B, use for metal or plastic inserts. Test before and after Dry Heat Age in section 4.5.1.2. Required: 600 N/m(width), foam failure only, adhesive failure shall be considered as
15、failing this test. 4.5.2 Integral Skin and In-mold Coating Properties shall be measured on a film cut from a molded part such that the thickness of the skin and included foam is 2.5 mm (0.1 inch) 0.25 mm (0.01 inch). 4.5.2.1 Tensile Test - ASTM D 412, Method 4, Die A: Required: Tensile Strength: 1.2
16、 MPa (180 psi) min Elongation: 80% min 4.5.2.2 Tear Resistance - ASTM D 624, D14 C: Required: 4.4kN/m (25 lbf per inch) minimum 4.5.2.3 Low Temperature Resistance - SAE J323, Method A, -32C (-25F) Required: Pass 4.5.2.4 Abrasion Resistance - ASTM D 3884, CS #10 Wheel, 500 gm load, 500 cycles Require
17、d: No appreciable loss of grain, texture, or any color change. NUMBER: TITLE: REVISION: TMS-6500 Cellular Polyurethane, Integral Skin 0810 This document is restricted and may not be sent outside Navistar, Inc. or reproduced without permission from Corporate Technical Standards. Suppliers are require
18、d to assume all patent liability. 2008 by Navistar, Inc. 4.5.2.5 Performance Requirements The following performance tests for the integral skin and coating may be performed on any convenient sample of the finish surface having thickness of not less than 2.5mm (0.1 inch). 4.5.2.5.1 Humidity - ASTM D
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- NAVISTARTMS65002008CELLULARPOLYURETHANEINTEGRALSKINPDF

链接地址:http://www.mydoc123.com/p-963477.html