1、Designation: D 4120 07Standard Test Method forFiber Cohesion in Roving, Sliver, and Top in Dynamic Tests1This standard is issued under the fixed designation D 4120; the number immediately following the designation indicates the year oforiginal adoption or, in the case of revision, the year of last r
2、evision. A number in parentheses indicates the year of last reapproval. Asuperscript epsilon (e) indicates an editorial change since the last revision or reapproval.1. Scope1.1 This test method describes the measurement of fibercohesion as the dynamic cohesive force required to maintaindrafting in r
3、ovings, slivers or tops when they are subjected tostress induced by passing between pairs of drafting rolls ofdifferent surface speeds. The cohesive force is converted tocohesive tenacity based on the linear density of the material.NOTE 1For static tests refer to Test Method D 2612.1.2 This standard
4、 does not purport to address all of thesafety concerns, if any, associated with its use. It is theresponsibility of the user of this standard to establish appro-priate safety and health practices and determine the applica-bility of regulatory limitations prior to use.2. Referenced Documents2.1 ASTM
5、Standards:2D 123 Terminology Relating to TextilesD 519 Test Method for Length of Fiber in Wool TopD 1440 Test Method for Length and Length Distribution ofCotton Fibers (Array Method)D 1447 Test Method for Length and Length Uniformity ofCotton Fibers by Fibrograph MeasurementD 1575 Test Method for Fi
6、ber Length of Wool in ScouredWool and in Card SliverD 1776 Practice for Conditioning and Testing TextilesD 2258 Practice for Sampling Yarn for TestingD 2612 Test Method for Fiber Cohesion in Sliver and Top(Static Tests)D 3333 Practice for Sampling Manufactured Staple Fibers,Sliver, or Tow for Testin
7、gD 4849 Terminology Relating to Yarns and Fibers3. Terminology3.1 For all terminology relating to D13.58, Yarns andFibers, refer to Terminology D 4849.3.1.1 The following terms are relevant to this standard:cohesive force, fiber cohesion, roving, sliver, tenacity, top.3.2 For all other terms are rel
8、ated to textiles, refer toTerminology D 123.4. Summary of Test Method4.1 This test method provides an indication of the ability offibers to hold together by measuring the force required to slidefibers in a direction parallel to their length. Specific lengths ofroving, sliver, or top are drafted betw
9、een two pairs of rollers,with each pair moving at a different peripheral speed. The draftforces are recorded. Test specimens are then weighed and thelinear density calculated. Drafting tenacity, calculated as thedraft resisting force per unit linear density, is considered to bea measure of the dynam
10、ic fiber cohesion.5. Significance and Use5.1 This test method for the determination of cohesion insliver, roving, or top in dynamic tests may be used for theacceptance testing of commercial shipments but caution isadvised since information on between-laboratory precision islacking. Comparative tests
11、 as directed in 5.1.1 may be advis-able.5.1.1 If there are differences or practical significance be-tween reported test results for two laboratories (or more),comparative test should be performed to determine if there is astatistical bias between them, using competent statistical assis-tance. As a m
12、inimum, test samples that are as homogeneous aspossible, drawn from the material from which the disparate testresults were obtained, and randomly assigned in equal numbersto each laboratory for testing. The test results from the two1This test method is under the jurisdiction of ASTM Committee D13 on
13、 Textilesand is the direct responsibility of Subcommittee D13.58 on Yarns and Fibers.Current edition approved Jan. 1, 2007. Published January 2007. Originallyapproved in 1982. Last previous edition approved in 2001 as D 4120 01.2For referenced ASTM standards, visit the ASTM website, www.astm.org, or
14、contact ASTM Customer Service at serviceastm.org. For Annual Book of ASTMStandards volume information, refer to the standards Document Summary page onthe ASTM website.1Copyright ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.laboratories shoul
15、d be compare using a statistical test forunpaired data, at a probability level chosen prior to the testingseries. If a bias is found either its cause must be found andcorrected, or future test results for that material must beadjusted in consideration of the known bias.5.2 The cohesive forces overco
16、me in continuous drafting ofslivers, rovings, or tops are affected by surface lubricants andsuch fiber properties as linear density, surface configuration,fiber length, fiber crimp, and fiber-frictional characteristics.5.2.1 The concept of drafting is one of the most importantprinciples in the produ
17、ction of yarn from fibrous raw stock.5.2.2 The values of force to maintain drafting determined bythis method are induced by mechanical means similar to thoseused in textile processing.5.2.3 The attenuation of textile fiber strands while in motionclosely approximates actual textile processing conditi
18、ons, andthe relative values of force may be used to predict processingbehaviors.5.3 Fiber cohesion is affected by the alignment of fiber inthe textile strand and strand compaction in addition to thefactors listed in 5.2. Although fibers are more nearly aligned indraw sliver than in card sliver, the
19、draw sliver is more compact.Thus, for a given production run, the drafting forces are higherfor draw sliver than for card sliver.5.4 In addition to the aforementioned effects on draftingforces, the direction of specimen movement through draftingrollers may give different drafting force. Fibers in sl
20、ivers mayhave hooks of varying severity at one or both ends. Passagethrough drafting rollers results in higher drafting forces whenthe predominance of fiber hooks are oriented in the trailingmode of the strand.6. Apparatus and Materials6.1 Cohesion Meter,3with rollers and controls for varyingdrafts
21、and rates of drafting.6.2 Tensiometer,3with accessory equipment includingmeasuring heads, integrator, (or computer or programmablecalculator), and recorder for sensing, accumulating, and re-cording drafting forces.6.3 Calibration Mass, 1 kg, NBS Class T.6.4 Tachometer, capable of measuring roll surf
22、ace speed towithin 0.1 m/min.6.5 Balance, with sufficient capacity and sensitivity toweigh specimens to within 0.1 % of specimen mass.7. Sampling7.1 Lot SamplingAs a lot sample for acceptance testing,take at random the number of shipping containers directed inthe applicable material specification or
23、 other agreement be-tween the purchaser and supplier, such as an agreement to usePractice D 3333 or Practice D 2258. Consider shipping con-tainers to be the primary sampling units.NOTE 2An adequate specification or other agreement between thepurchaser or supplier requires taking into account the var
24、iability betweenshipping units, between packages, ends or other laboratory sampling unitwithin a shipping unit if applicable, and within specimens from a singlepackage, end or other laboratory sampling unit to provide a sampling planwith a meaningful producers risk, consumers risk, acceptable qualit
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- ASTMD41202007STANDARDTESTMETHODFORFIBERCOHESIONINROVINGSLIVERANDTOPINDYNAMICTESTS 动态 试验 下粗纱 毛条 纤维 粘附

链接地址:http://www.mydoc123.com/p-516318.html