ASTM D2674-1972(2012) Standard Methods of Analysis of Sulfochromate Etch Solution Used in Surface Preparation of Aluminum《铝表面处理用硫代铬酸盐蚀刻溶液分析的标准试验方法》.pdf
《ASTM D2674-1972(2012) Standard Methods of Analysis of Sulfochromate Etch Solution Used in Surface Preparation of Aluminum《铝表面处理用硫代铬酸盐蚀刻溶液分析的标准试验方法》.pdf》由会员分享,可在线阅读,更多相关《ASTM D2674-1972(2012) Standard Methods of Analysis of Sulfochromate Etch Solution Used in Surface Preparation of Aluminum《铝表面处理用硫代铬酸盐蚀刻溶液分析的标准试验方法》.pdf(3页珍藏版)》请在麦多课文档分享上搜索。
1、Designation: D2674 72 (Reapproved 2012)Standard Methods ofAnalysis of Sulfochromate Etch Solution Used in SurfacePreparation of Aluminum1This standard is issued under the fixed designation D2674; the number immediately following the designation indicates the year oforiginal adoption or, in the case
2、of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. Asuperscript epsilon () indicates an editorial change since the last revision or reapproval.1. Scope1.1 These methods offer a means for controlling the effec-tiveness of the etchant which is normal
3、ly used for preparing thesurface of aluminum alloys for subsequent adhesive bonding.As the etchant reacts with the aluminum, hexavalent chromiumis converted to trivalent chromium; a measure of the two andthe difference can be used to determine the amount of dichro-mate used.1.2 The sulfochromate sol
4、ution can be replenished by re-storing the sodium dichromate and the sulfuric acid to theoriginal formulation levels. The lower limit of usefulness willvary depending upon solution storage, adhesives used, criticalnature of bond capability, variety of metals processed, etc. andshould be determined.
5、Replenishment will be limited to thenumber of times the chemical ingredients can be restored andmaintained to the required levels and should be determined bythe user. Sludge collecting in the bottom of a tank should beminimized by periodic removal of sludge. For some applica-tions, the hexavalent ch
6、romium should not fall below thetrivalent chromium content.1.3 A typical aqueous sulfochromate acid etch solutionformulation is as follows:Sodium dichromate (Na2Cr2O7) 4.5 oz/gal (33.7 g/litre)Sulfuric acid (sp gr 1.84) 45 oz/gal (337.1 g/litre)1.4 Maintenance of the aqueous concentrations is sugges
7、tedas follows by appropriate additions of sodium dichromate orsulfuric acids.Sodium dichromate 3.0 to 6.0 oz/gal (22.5 to 44.9 g/litre)Sulfuric acid 40 to 50 oz/gal (299.6 to 374.5 g/litre)1.5 Method A is intended for measuring the sulfuric acidcontent of a sulfochromate solution. Method B is intend
8、ed formeasuring the hexavalent and trivalent Chromium content of asulfochromate solution. Method C is intended as an alternativemethod for measuring the hexavalent and trivalent Chromiumcontent of a sulfochromate solution.1.6 This standard does not purport to address all of thesafety concerns, if an
9、y, associated with its use. It is theresponsibility of the user of this standard to establish appro-priate safety and health practices and determine the applica-bility of regulatory limitations prior to use.2. Referenced Documents2.1 ASTM Standards:2D1193 Specification for Reagent WaterE50 Practices
10、 for Apparatus, Reagents, and Safety Consid-erations for Chemical Analysis of Metals, Ores, andRelated Materials3. Purity of Reagents and Water3.1 Purity of ReagentsReagent grade chemicals shall beused in all tests. Unless otherwise indicated, it is intended thatall reagents shall conform to the spe
11、cifications of the Commit-tee on Analytical Reagents of the American Chemical Society,where such specifications are available.3Other grades may beused, provided it is first ascertained that the reagent is ofsufficiently high purity to permit its use without lessening theaccuracy of the determination
12、.3.2 Purity of WaterUnless otherwise indicated, referencesto water shall be understood to mean reagent water conformingto Specification D1193.METHOD A4. Apparatus4.1 pH Meter.5. Reagents5.1 Methyl Orange Indicator SolutionPrepare in accor-dance with Practices E50.1These methods are under the jurisdi
13、ction of ASTM Committee D14 onAdhesives and are the direct responsibility of Subcommittee D14.80 on MetalBonding Adhesives.Current edition approved May 1, 2012. Published May 2012. Originallyapproved in 1967. Last previous edition approved in 2004 as D2674 72 (2004)1.DOI: 10.1520/D2674-72R12.2For re
14、ferenced ASTM standards, visit the ASTM website, www.astm.org, orcontact ASTM Customer Service at serviceastm.org. For Annual Book of ASTMStandards volume information, refer to the standards Document Summary page onthe ASTM website.3Reagent Chemicals, American Chemical Society Specifications, Americ
15、anChemical Society, Washington, D.C. For suggestions on the testing of reagents notlisted by the American Chemical Society, see Analar Standards for LaboratoryChemicals, BDH Ltd., Poole, Dorset, U.K., and the United States Pharmacopeiaand National Formulary, U.S. Pharmacopeial Convention, Inc., (USP
16、C), Rockville,MD.1Copyright ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.5.2 Sodium Hydroxide, Standard Solution (1.0 N)Dissolve 40 g of sodium hydroxide (NaOH) in 1 liter of waterand standardize.6. Procedure6.1 Pipet a 5-mL sample of sulfoc
17、hromate etch solution intoa 250-mL beaker.Add 100 mL of water. Titrate the sample withthe NaOH solution to a pH of 3.5, using a pH meter.6.2 An alternative method may be used whereby, instead ofthe pH meter, 1 drop of methyl orange indicator solution isadded and, the titration continued until the co
18、lor of the solutionloses all trace of orange.7. Calculation7.1 Calculate the sulfuric acid content of the sulfochromatesolution, A in oz/gal, B in g/litre, as follows:A 5 1.3 VN (1)B 5 9.81 VN (2)where:V = milliliters of sodium hydroxide solution, andN = normality of sodium hydroxide solution.7.2 Re
19、plenish the sulfuric acid content of the solution asfollows:W15 A12 A!V1(3)W25 B12 B!V2(4)where:W1= weight of sulfuric acid (H2SO4, sp gr 1.84) to beadded to solution, oz,W2= weight of sulfuric acid to be added to solution, g,A1= original concentration of solution, oz/gal,B1= original concentration
20、of solution, g/litre,V1= volume of solution in tank, gal, andV2= volume of solution in tank, litres.METHOD B8. Reagents8.1 Ammonium Persulfate Solution (NH4)2SSO8, 15weight %).8.2 Ferrous Ammonium Sulfate Solution (0.05 N)Dissolve 39.2 g of ferrous ammonium sulfate(Fe(NH4)2(SO4)26H2O) in 1 litre of
21、cold H2SO4(5 + 95) anddilute to 2 litres with H2SO4(5 + 95). Standardize this materialeach time as follows:8.2.1 Pipet 10 mL into a 400-mL beaker. Add 150 mL ofwater plus 5 mL of H2SO4(sp gr 1.84) and 1 drop of thephenanthroline ferrous complex. Titrate with the KMnO4solution just to disappearance o
22、f the indicator color. If thenormality does not fall within 0.051 to 0.049, discard the 0.05N solution.8.3 Hydrochloric Acid (1 + 1)Mix 1 volume of concen-trated hydrochloric acid (HCl) with 1 volume of water.8.4 Ortho-Phenanthroline Ferrous Complex IndicatorSolutionPrepare in accordance with Practi
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- ASTMD267419722012STANDARDMETHODSOFANALYSISOFSULFOCHROMATEETCHSOLUTIONUSEDINSURFACEPREPARATIONOFALUMINUM

链接地址:http://www.mydoc123.com/p-513301.html