RCC-M-Edition 2007 SECTION I:SUBSECTION Z TECHNICAL APPENDICES.pdf
《RCC-M-Edition 2007 SECTION I:SUBSECTION Z TECHNICAL APPENDICES.pdf》由会员分享,可在线阅读,更多相关《RCC-M-Edition 2007 SECTION I:SUBSECTION Z TECHNICAL APPENDICES.pdf(289页珍藏版)》请在麦多课文档分享上搜索。
1、RCC-M-Edition 2007 SECTION I:SUBSECTION Z TECHNICAL APPENDICES_TECHNICAL APPENDICESSECTION I : SUBSECTION Z DESIGN AND CONSTRUCTION RULESFOR MECHANICAL COMPONENTS OF PWRNUCLEAR ISLANDSRCC-MRCC-M - Edition 2007 Subsection Z n 113-2007 Annex ZI / 1 ANNEX Z I PROPERTIES OF MATERIALS TO BE USED IN DESIG
2、N Tables Z I 1.0 ALLOWABLE BASIC STRESS INTENSITY VALUES SmALLOWABLE BASIC STRESS VALUES S Table Z I 1.1 Allowable basic stress intensity values Sm for ferritic steels Table Z I.1.2 Allowable basic stress intensity values Sm for stainless steels and Ni-Cr-Fe alloys Table Z I.1.3 Allowable basic stre
3、ss intensity values Sm for bolting materials Table Z I.1.4 Allowable basic stress values S for ferritic steels Table Z I.1.5 Allowable basic stress values S for stainless steels and Ni-Cr-Fe alloys Table Z I.1.6 Allowable basic stress values S for bolting materials Tables Z I 2.0 YIELD STRENGTH VALU
4、ES Sy Table Z I 2.1 Yield strength values Sy for ferritic steels Table Z I.2.2 Yield strength values Sy for stainless steels and Ni-Cr-Fe alloys Table Z I.2.3 Permanent strain limiting factors Tables Z I 3.0 TENSILE STRENGTH VALUES Su Table Z I 3.1 Tensile strength values Su for ferritic steels Tabl
5、e Z I.3.2 Tensile strength values Su for stainless steels and Ni-Cr-Fe alloys Figures Z I 4.0 FATIGUE CURVES Figure Z I 4.1 Fatigue curves for carbon and low alloy steels Figure Z I.4.2 Fatigue curves for austenitic steels and nickel alloys Figure Z I.4.3 Fatigue curves for steel bolting Table Z I 5
6、.0 CLASSIFICATION OF THE VARIOUS GRADES USED IN THE RCC-M FOR PHYSICAL PROPERTIES Table Z I 6.0 a THERMAL CONDUCTIVITY Table Z I 6.0 b THERMAL DIFFUSIVITY Table Z I 7.0 COEFFICIENTS OF LINEAR EXPANSION Table Z I 8.0 MODULUS OF ELASTICITY RCC-M - Edition 2007 Subsection Z Annex ZI /2 n 113-2007 TABLE
7、 Z I 1.1 ALLOWABLE BASIC STRESS INTENSITY VALUES Sm FOR FERRITIC STEELS 370C 132 132 117 132 - - - - - - - - - - - - - - - - - - - - - 360C 133 133 117 133 - - - - - - - - - - - - - - - - - - - - - 350C 133 133 117 133 - - 95 117 95 117 - - 79 79 95 95 117 117 137 137 - - - - - 340C 134 134 117 134
8、- - 96 121 96 121 - - 79 79 96 96 121 121 138 138 - - - - - 300C 139 139 122 139 - - 105 131 105 131 124 124 85 85 105 105 131 131 144 144 91 107 137 124 124 250C 151 151 133 151 - - 117 144 117 144 144 144 98 98 117 117 144 144 157 157 103 120 155 144 144 200C 158 158 139 158 - - 124 147 124 147 15
9、7 157 111 105 127 124 157 147 170 170 113 133 163 157 157 150C 161 161 141 161 183 183 127 153 127 153 157 157 120 111 137 127 157 153 170 170 113 133 163 157 157 100C 161 161 141 161 183 183 134 157 134 157 157 157 120 120 137 134 157 157 170 170 113 133 163 157 157 ALLOWABLE BASIC STRESS INTENSITY
10、 VALUES SmIN MPa 50C 161 161 141 161 183 183 137 157 137 157 157 157 120 120 137 137 157 157 170 170 113 133 163 157 157 Suat 20C 483 483 470 483 550 550 410 470 410 470 470 470 360 360 410 410 470 470 510 510 340 400 470 470 470 Syat 20C 241 241 212 241 345 345 215 255 215 255 275 275 225 185 245 2
11、15 285 255 335 305 235 275 355 275 275 MIN Rm in Mpa at 20C 485 485 470 485 550 550 410 460 410 470 470 470 360 360 410 410 470 470 510 510 340 400 470 470 470 MIN Re in Mpa at 20C 275 275 235 275 345 345 215 255 215 255 275 275 225 185 245 215 285 255 335 305 235 275 355 275 275 DIMENSION (mm) e 30
12、 e 30 e 30 e 30 e 30 e 30 e 30 e 30 3 e 30 3 e 30 3 e 30 AFNOR GRADE 20 MN 5M 20 MN 5M 20 M 5M 20 MN 5M 23 M 5M 20 CD 4M P 245 GH P 265 GH P 280 GH P 295 GH A 42 A 48 P 280 GH P 280 GH P 235 GH P 265 GH P 295 GH P 355 GH S 235 S 275 S 355 P 280 GH P 280 GH PRODUCT FORM Casting Casting Casting Castin
13、g Forging (0) Forging (0) Rolled or Forging Forging elbow Plate Plate Pipe Pipe TPS* M 1111 M 1112 M 1114 M 1115 M 1122 M 1122 bis M 1124 M 1125 M 1131 M 1132 M 1134 M 1144 M 1152 * TPS : Technical Procurement Specification RCC-M - Edition 2007 Subsection Z n 113-2007 Annex ZI /3 TABLE Z I 1.1 (Cont
14、.) ALLOWABLE BASIC STRESS INTENSITY VALUES Sm FOR FERRITIC STEELS 370C 184 184 193 200 193 200 - - 360C 184 184 193 200 193 200 - - 350C 184 184 193 200 193 200 - - 340C 184 184 193 200 193 200 - - 300C 184 184 193 200 193 200 - - 250C 184 184 193 200 193 200 - - 200C 184 184 193 200 193 200 - - 150
15、C 184 184 193 200 193 200 - - 100C 184 184 193 200 193 200 183 250 ALLOWABLE BASIC STRESS INTENSITY VALUES SmIN MPa 50C 184 184 193 200 193 200 183 250 Suat 20C 552 552 580 600 580 600 550 750 Syat 20C 345 345 420 450 420 435 280 600 MIN Rm in Mpa at 20C 550 550 580 600 580 600 550 750 MIN Re in Mpa
16、 at 20C 400 400 420 450 420 450 280 600 DIMENSION (mm) 125 125 (1) AFNOR GRADE 16 MND 5 16 MND 5 18 MND 5 18 MND 5 18 MND 5 30 M 5 20 NDC 14.07 PRODUCT FORM Forging Plate Forging Forging Plate Forging Plate TPS* M 2111 M 2111 Bis M 2112 M 2112 Bis M 2113 M 2114 M 2115 M 2116 M 2117 M 2119 M 2131 M 2
17、141 M 2142 M 2143 M 2121 M 2122 M 2125 M 2126 M 2127 M 2115 M 2143 M 2119 M 2133 M 2134 M 2125 M 2126 M 2127 M 2128 M 2132 M 2321 Notes : (0) The values indicated cover thicknesses up to 110 mm (1) This limit can be increased up to 160 mm by special agreement when the order is placed * TPS : Technic
18、al Procurement Specification RCC-M - Edition 2007 Subsection Z Annex ZI /4 n 113-2007 TABLE Z I 1.2 ALLOWABLE BASIC STRESS INTENSITY VALUES SmFOR STAINLESS STEELS AND Ni-Cr-Fe ALLOYS 370C 161 229 225 110 110 110 110 93 93 110 110 128 128 110 110 112 112 112 112 89 89 360C 163 229 226 111 111 111 111
19、 94 94 111 111 129 129 111 111 113 113 113 113 90 90 350C 165 229 228 111 111 111 111 94 94 111 111 130 130 111 111 114 114 114 114 90 90 340C 166 229 229 111 111 111 111 94 94 111 111 131 131 112 112 115 115 115 115 91 91 300C 170 233 234 115 115 115 115 97 97 115 115 134 134 115 115 119 119 119 11
20、9 95 95 250C 175 240 238 122 122 122 122 102 102 122 122 137 137 122 122 126 126 126 126 100 100 200C 176 244 242 130 130 130 130 109 109 130 130 138 138 130 130 134 134 134 134 108 108 150C 180 247 247 138 138 138 138 114 114 138 138 138 138 138 138 138 138 138 138 115 115 100C - 252 252 138 138 13
21、8 138 114 114 138 138 138 138 138 138 138 138 138 138 115 115 ALLOWABLE BASIC STRESS INTENSITY VALUES SmIN MPa 50C 183 253 253 138 138 138 138 114 114 138 138 138 138 138 138 138 138 138 138 115 115 Suat 20C 550 758 758 517 483 517 483 483 448 517 483 517 483 517 483 517 483 517 483 483 448 Syat 20C
22、 400 620 552 in preparation in preparation 207 207 173 207 207 207 207 207 173 MIN Rm in Mpa at 20C 550 760 760 540 900 520 485 520 485 490 450 520 485 540 490 540 490 520 485 520 485 490 450 MIN Re in Mpa at 20C 400 620 550 380 720 210 210 175 210 220 220 210 210 175 DIMENSION (mm) 550 550 ? 150 ?
23、150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 ? 150 AFNOR GRADE Z10 C13 Z12 CN13 Z5 CND 13.04 Z5 CN 12.01 Z6 CNU 17.04 Z6 CN 18.10 Z5 CN 18.10 Z2 CN 18.10 Z2 CN 19.10 controlled nitrogen content Z6 CNNb 18.11 Z8 CNT 18.11 Z6 CND 17.12 Z5 CND 17.12 Z2 C
24、ND 17.12 PRODUCT FORM Plate Forging Casting Forging (1) (2) Rolled bar (1) (2) TPS* M 3203 M 3205 M 3208 M 3301 M 3306 * TPS : Technical Procurement Specification RCC-M - Edition 2007 Subsection Z n 113-2007 Annex ZI /5 TABLE Z I 1.2 (Cont. 1) ALLOWABLE BASIC STRESS INTENSITY VALUES SmFOR STAINLESS
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- RCC Edition 2007 SECTION SUBSECTION TECHNICAL APPENDICES

链接地址:http://www.mydoc123.com/p-11844.html