FORD WSS-M2D507-B5-2016 THERMOPLASTIC ELASTOMER (TPS) STYRENE BLOCK COPOLYMER 80 DUROMETER A HARDNESS INTERIOR TO BE USED WITH FORD WSS-M99P1111-A (Shown on FORD WSS-M2D507-B4).pdf
《FORD WSS-M2D507-B5-2016 THERMOPLASTIC ELASTOMER (TPS) STYRENE BLOCK COPOLYMER 80 DUROMETER A HARDNESS INTERIOR TO BE USED WITH FORD WSS-M99P1111-A (Shown on FORD WSS-M2D507-B4).pdf》由会员分享,可在线阅读,更多相关《FORD WSS-M2D507-B5-2016 THERMOPLASTIC ELASTOMER (TPS) STYRENE BLOCK COPOLYMER 80 DUROMETER A HARDNESS INTERIOR TO BE USED WITH FORD WSS-M99P1111-A (Shown on FORD WSS-M2D507-B4).pdf(6页珍藏版)》请在麦多课文档分享上搜索。
1、 ENGINEERING MATERIAL SPECIFICATION Date Action Revisions Rev. 1 2016 01 11 Revised See Summary of Revisions T.Nover, EU 2014 12 08 Released T.Nover, M.Corley, EU Controlled document at www.MATS Copyright 2016, Ford Global Technologies, LLC Page 1 of 6 THERMOPLASTIC ELASTOMER (TPS) WSS-M2D507-B4 STY
2、RENE BLOCK COPOLYMER, 70 DUROMETER A HARDNESS, INTERIOR THERMOPLASTIC ELASTOMER (TPS) WSS-M2D507-B5 STYRENE BLOCK COPOLYMER, 80 DUROMETER A HARDNESS, INTERIOR 1. SCOPE The material defined by this specification is a thermoplastic elastomer based on styrene block copolymer. 2. APPLICATION These speci
3、fications were released originally for material used for interior applications. Typical applications are mats (cupholder, bin) or thumb wheels. 2.1 LIMITATONS These specifications should be only used for applications with minimal compression set requirements. 3. REQUIREMENTS 3.1 APPROVED SOURCES Thi
4、s specification requires the use of approved sources. Only the sources identified on the Ford Approved Source List (ASL) can be used when this specification is listed on the drawing, CAD file, or other documents. The list of approved sources is located within Ford at or available externally through
5、 a Ford Materials Engineer. 3.2 CONDITIONING AND TEST CONDITIONS All test values are based on material conditioned for not less than 24 h prior to testing in a controlled environment of 23 +/- 2 C and 50 +/- 5% relative humidity. Testing of the material should occur in the conditioning environment o
6、r soon after removal. 3.3 STANDARD REQUIREMENTS FOR PRODUCTION MATERIALS 3.3.1 The use of regrind is permitted, for economic / environmental reasons, with compliance as indicated in Ford Engineering CAD and Drafting Standard E-4 3.3.2 Materials used in interior applications must meet the requirement
7、s outlined in WSS-M99P2222-D1/Latest, Performance, Vehicle Interior Environment Quality Material/Component Requirements. Data must be included in material submission package. 3.3.3 Performance Criteria: Parts using this specification shall meet the appropriate performance specifications, WSS-M9P8-C/
8、Latest. ENGINEERING MATERIAL SPECIFICATION WSS-M2D507-B4 WSS-M2D507-B5 Copyright 2016 Ford Global Technologies, LLC Page 2 of 6 3.4 APPEARANCE 3.4.1 Xenon Arc Weatherometer Rating 4 min (FLTM BO 116-01, 2406,4 kJ/m exposure minimum, specimen size: 150 x, 100 mm minimum, 2.0 +/- 0.2 mm thick molded i
9、n smooth polished mold) 3.5 MATERIAL PROPERTIES 3.5.1 Density Report Only, g/cm3 (ISO 1183-1, Method A) 3.5.2 Hardness (ISO 868, 6 mm piled-up specimen, 15 seconds dwell) B4 70 +/-5 Shore A B5 80 +/-5 Shore A 3.5.3 Tensile Strength at Break (ISO 37, Type 2 specimen, 75 x 4 x 2.0 +/- 0.2 mm 500 mm/mi
10、nute test speed) 3.5.3.1 Parallel to Flow B4 4.0 MPa min B5 5.0 MPa min 3.5.3.2 Perpendicular to flow B4 4.5 MPa min B5 5.5 MPa min 3.5.4 Elongation at Break (ISO 37, Type 2 Specimen at 500 mm/min) 3.5.4.1 Parallel to Flow B4 400 % min B5 400 % min 3.5.4.2 Perpendicular to flow B4 500 % min B5 500 %
11、 min 3.5.5 Tensile Modulus at 100 % Elongation (ISO 37, Type 2 Specimen at 500 mm/min) 3.5.5.1 Parallel to Flow B4 1.5 MPa min B5 2.0 MPa min 3.5.5.2 Perpendicular to flow B4 2.0 MPa min B5 2.5 MPa min ENGINEERING MATERIAL SPECIFICATION WSS-M2D507-B4 WSS-M2D507-B5 Copyright 2016 Ford Global Technolo
12、gies, LLC Page 3 of 6 3.5.6 Tear Strength (unnotched tear) (ISO 34-1, Method B, Procedure A / ASTM D624, Die C) 3.5.6.1 Parallel to Flow B4 22 kN/m min B5 25 kN/m min 3.5.6.2 Perpendicular to flow B4 24 kN/m min B5 27 kN/m min 3.5.7 Low Temperature Brittleness No Cracking (ISO 812, Type B Specimen/
13、ASTM D2187, Method A, at -40 C) 3.5.8 Ozone Resistance 0 Rating (FLTM BP 101-01, Procedure A, tensile specimen, 20% Elongation) 3.5.9 Fogging, Photometric (SAE J1756, 3 h at 100 C heating, 21C Cooling Plate, post test conditioning 1 h and 16 h) Fog Number 70, min 3.5.10 Odor Rating 3, max (FLTM BO 1
14、31-03) 3.5.11 Stain Resistance (Migration) Rating 5 (FLTM BN 103-01, ISO 105-A02/ AATCC Evaluation Procedure 2) No evidence of exudation, adhesion (tackiness), separation, color transfer, or flattening of embossing when placed face to face with itself. 3.5.12 Heat Aging (ISO 188, except 150 +/- 50 a
15、ir changes/h, 1000 h at 100 C +/- 2C) 3.5.12.1 Hardness Change (Test Method per para 3.5.2) B4 +/-5 B5 +/-5 3.5.12.2 Tensile Strength Change +/- 25 % (Test Method per para 3.5.3) 3.5.12.3 Elongation Change +/- 25 % (Test Method per para 3.5.4) 3.5.12.4 Brittleness or Bend Test No Cracks (Test Method
16、 per para 3.5.7) ENGINEERING MATERIAL SPECIFICATION WSS-M2D507-B4 WSS-M2D507-B5 Copyright 2016 Ford Global Technologies, LLC Page 4 of 6 3.5.13 Coefficent of Linear Thermal Expansion, mm C x 1-5 (ISO 11359-2) Flow Direction (Machine Direction) Report Transverse to Flow (Cross Machine) Report 3.5.14
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- FORDWSSM2D507B52016THERMOPLASTICELASTOMERTPSSTYRENEBLOCKCOPOLYMER80DUROMETERAHARDNESSINTERIORTOBEUSEDWITHFORDWSSM99P1111ASHOWNONFORDWSSM2D507B4PDF

链接地址:http://www.mydoc123.com/p-752880.html