FORD WSB-M18P15-A-1993 SEALING REQUIREMENTS NON DRYING MASTIC SEALED LAMP SOCKETS《密封灯座的非干燥胶泥的密封性能要求》.pdf
《FORD WSB-M18P15-A-1993 SEALING REQUIREMENTS NON DRYING MASTIC SEALED LAMP SOCKETS《密封灯座的非干燥胶泥的密封性能要求》.pdf》由会员分享,可在线阅读,更多相关《FORD WSB-M18P15-A-1993 SEALING REQUIREMENTS NON DRYING MASTIC SEALED LAMP SOCKETS《密封灯座的非干燥胶泥的密封性能要求》.pdf(5页珍藏版)》请在麦多课文档分享上搜索。
1、 ENGINEERING MATERIAL SPECIFICATIONMaterial Name Specification NumberDate Release No. Release/Revision1993 10 01 NB00I10043054285 Released W.Curtiss E.Rezendes M.PerchardWP 3948-a Page 1 of 5 SEALING REQUIREMENTS, NON-DRYING MASTIC, WSB-M18P15-ASEALED LAMP SOCKETS1. SCOPEThi s specification defines
2、the sealing requirements for specific sealedlamp s ocket applications using a non-drying, asbestos-free mastic pottingcompou nd consisting of a synthetic and natural oil base with other fillermaterials.2. APPLICATIONThis spe cification was released originally for material used as a masticsea ler in
3、lamp socket applications to provide sealing properties whenexposed to weathering condition s on vehicles. This material does not dry,crack or sag after extended use and is compatible with the socketcomponents to which it comes in contact.3. REQUIREMENTS3.1 STATISTICAL PROCESSSupplie rs must conform
4、to the requirements of Ford Quality SystemStand ard Q-101. A mutually acceptable Control Plan as describedtherein is required for material/source approval. Appropriatestatist ical tools must be used to analyze process/product data sothat variation in the final product is continuously reduced.3.2 INF
5、RARED SPECTROPHOTOMETRY AND/OR THERMAL ANALYSISFord Motor Company, at its option, may conduct infrared and/ortherma l analysis of material/parts supplied to this specification.The IR spectra and thermograms established for i nitial approval shallconst itute the reference standard and shall be kept o
6、n file at thedesignated material laboratory. All samples sha ll produce IR spectraand thermograms that correspond to the reference standard when testedunder the same conditions.3.3 CONDITIONING AND TEST CONDITIONSAll test values indicated herein are based on ma terial conditioned ina control led atm
7、osphere of 23 +/- 2 C and 50 +/- 5 % relativehumidity for not less than 24 h prior to testing and tested under thesame conditions unless otherwise specified.ENGINEERING MATERIAL SPECIFICATIONWSB-M18P15-AWP 3948-b Page 2 of 5 3.4 SAG AND WEATHERING RESISTANCESha ll not sag, dry, crack or separate oil
8、 when subjected to thefollowing conditions.3.4.1 2 h at - 40 +/- 1 C3.4.2 2 h at 93 +/- 1 C3.4.3 100 h at 70 +/- 1 CTest Method:. Prepare and test a minimum of three test panels per testcondition. Apply a ribbon of ma terial 13 x 200 x 7 mm to a clean CRSpanel. Cut off the ribbon on both ends to eli
9、minate necking. Scribe the panel to mark the initial position of thematerial. Position the panel horizontally and subject the panel tothe environments listed above. Examine the panel after the exposure and note anydeleterious effects.3.5 EXPANSION/SHRINKAGETest Temperature Volume Expansion/Shrinkage
10、3.5.1 At 49 +/- 2 C 0 - 6 %Recovery to 23 +/- 2 C 0 - 2 %3.5.2 At 100 +/- 2 C 5 - 15 %Recovery to 23 +/- 2 C 0 - 2 %Test Method:. Fill an ointment tin (53 mm O.C. x 40 mm deep) with thetest material. Avoid entrapment of air. Record the depth of the test material prior to exposure(D1) within +/- 1 mm
11、. Expose the prepared sample to the above test temperaturesfor 1 h, 6 h, and 6 days. Immediately upon removal from the test temperature, measurethe height of the test material (D2). Allow the sample to cool to 23 +/- 2 C for 4 h minimum andmeasure the material height (D3).ENGINEERING MATERIAL SPECIF
12、ICATIONWSB-M18P15-AWP 3948-b Page 3 of 5 . Record % Volume Expansion/Shrinkage of material immediatelyupon removal from test temperature and after sample hascooled to 23 +/- 2 C.% Volume Expansion/Shrinkage = (D2 or D3) - D1 x 100D13.6 TEMPERATURE OF EXPANSION Material shall not foam below 95 CTest
13、Method:. Fill an ointment tin (53 mm O.D. x 40 mm deep) with the testmaterial. Avoid entrapment of air. Place the sample in an oven at 50 +/- 2 C for 30 minutes. Raise the oven temperature 15 +/- 2 C every 15 minutes and visuallyinspect for signs of foaming or expansion at the end of each 15minute p
14、eriod. Discontinue test when foaming or expansion occurs or aftercompletion of exposure period at 110 +/- 2 C. Record the temperature at which foaming occurs or indicate “NoFoaming“.3.7 LOW TEMPERATURE FLEXIBILITY Material shall not crackTest Method:. Apply a ribbon of sealer 13 x 200 x 7 mm to alum
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制: