1、MIL-B-4434b 83 M 7777906 0403506 3 M t I MIL-B-44346(GL) 24 by 1989 MILITARY SPECIFICATION BATTING, SYNTHETIC FIBER, MEDIUM DENSITY This specification is approved for use by the Natick Research, Development, and Engineering Center, Department of the Army, and is available for use by all Departments
2、and Agencies of the Department of Defense. 1. SCOPE 1.1 Scope. This specification covers one type of polyester fiber batting material. 2. APPLICABLE DOCUMENTS 2.1 Government documents. 2.1.1 Specifications, standards, and handbooks. The following specifi- cations, standards, and handbooks form a par
3、t of this document to the extent specified herein. Unless otherwise specified, the issues of these documents are those listed in the issue of the Department of Defense Index of Specifi- cations and Standards (DODISC) and supplement thereto, cited in the solicitation (see 6.2). SPECIFICATIONS FEDERAL
4、 PPP-P-1133 - Packaging of Synthetic Fiber Fabrics -. r; i Beneficial comments (recommendations, additions, deletions) and any pertinent data which may be of use in improving this document should be addressed to: U.S. Army Natick Research, Development, and Engineering Center, Natick, MA 01760-5014 b
5、y using the self-addressed Standardization Document Improvement Proposal (DD Form 1426) appearing at the end of this document or by letter. AMSC N/A FSC 8320 DISTRIBUTION STATEMENT A. Approved for public release; distribution is unlimited. THIS DOCUMENT CONTAINS /o PAGES. Provided by IHSNot for Resa
6、leNo reproduction or networking permitted without license from IHS-,-,-_- MIL-B-4431b 83 M 7779706 0103507 5 MIL-B-44346 (GL) MILITARY MIL-C-21852 - Cloth, Taffeta, Nylon STANDARDS FEDERAL FED-STD-191 - Textile Test Methods MILITARY MIL-STD-105 - Sampling Procedures and Tables for Inspection by Attr
7、ibutes (Unless otherwise indicated, copies of federal and miiitary specifications, standards, and handbooks are available from the Naval Publications and Forms Center, (ATTN: NPODS), 5801 Tabor Avenue, Philadelphia, PA 19120-5099.) 2.2 Non-Government publications, The following document forms a part
8、 of this document to the extent specified herein. Unless otherwise specified, the issues of the documents which are DOD adopted shall be those listed in the issue of the DODISS cited in the solicitation. Unless otherwise specified, the issues of documents not: listed in the DODISS are the issues of
9、the documents cited iri the solicitation (see 6.2). AMERICAN ASSOCIATION OF TEXTILE CHEMISTS AND COLORISTS (AATCC) AATCC - 135 Test Method for Dimensional Changes in Automatic Home Laundering of Woven and Knitted Fabrics (Application for copies should be addressed to the American Association of Text
10、ile Chemists and Colorists, P.O. Box 12215, Research Triangle Park, NC 27709-2215.) (Non-Government standards and other publications are normally available from the organizations that prepare or distribute the documents. These documents also may be available in or through libraries or other informat
11、ional services.) 2.3 Order of precedence. In the event of a conflict between the text of this document and the references cited herein, the text of this document takes precedence. Noth.ing in this document, however, supersedes applicable laws and regulations unless a specific exemption has been obta
12、ined. 3, REQUIREMENTS 3.1 First article. When specified (see 6.2), a sample shall be subjected to first article inspection (see 6.3) in accordance with 4.3. 2 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-MIL-B-4434b 83 H 79779Ob 0403508 7 W 1 3.2
13、Materials. 3.2.1 Polyester binder fiber, 4.0 denier. The fiber shall be 4.0 denier and shall consist of a core of polyester having a minimum melting point of 465OF sheathed with polyester polymer mixture having a melting point of 2750 to 3OOOF. The core and sheath shall each make up 50 +/- 10 percen
14、t by weight of the fiber. The fiber shall have 8 to 10 crimps per inch and a 1.5 to 2.0 inch cut staple length. 3.2.2 Polyester fiber, 1.65 denier. The fiber shall be 1.65 denier and shall be formed from polyester having a minimum melting point of 465OF. The iber shall have 8 to 10 crimps per inch a
15、nd a 1.5 to 2.0 inch cut staple length. 3.2.3 Polyester fiber, 1.65 denier, coated. The fiber shall be 1.65 denier and shall be formed from polyester having a minimum melting point of 4650F. The fiber shall be coated with a durable-polydimethyl-siloxane such that 0.25 to 0.55 percent by weight of th
16、e coated fiber will be silicone. The fiber shall have 8 to 10 crimps per inch and a 1.5 to 2.0 inch cut staple length, 3.3 Construction. 3,3,1 FiSer blend. The polyester fibers specified in 3.2.1, 3.2.2, and 3,2,3 shall be intimately blended in the following proportions: Fiber 4.0 denier (3.2.1) 1.6
17、5 denier (3.2.2) 1.65 denier, coated (3.2.3) Percent o blend (+/- 5) 25 37.5 37.5 3.3.2 Batting fabrication. The intimate fiber blend specified in 3.3.1 shall be made into batting by air-laying or card/cross lapping fibers into a web which is then consolidated by needlepunching to achieve the battin
18、g weight and thickness requirements specified in table I. The consolidated batting shall be heat set to bond the fibers. A timeltemperature exposure shall be established for heat treatment which enables the binder fibers in the batting center to be activated without providing excessive heat exposure
19、 (excessive heat exposure can result in a harsh surface hand). 3.4 Physical requirements. The finished bonded batting shall conform to the requirements specified in table I, 3.4.1 and 3.4.2 when tested as speci- fied in 4.4.3. Provided by IHSNot for ResaleNo reproduction or networking permitted with
20、out license from IHS-,-,-MIL-B-443Lib 83 797990b 0403509 9 I TABLE I. Physical requirements Characteristic Requirement Weight, oz/yd2 8.4 +/- 0.8 Thickness, inches, at 0.002 psi, min: ini tia1 after laundering Dimensional stability, percent, max: length and width O. 63 O. 57 _ 3.4.1 Batting evenness
21、. The evenness of the finished bonded batting shall be such that no single weight determination shall deviate more than 10 percent from the 8.4 oz/yd2 target weight specified in table I. specimen shall be used for each weight determination. specified in 4.4.3. A 12 by 12-inch Testing shall be as 3.4
22、.2 Launderabil-ity. The laundered batting shall show no greater batting separation, thin or thick spots, or curling than the batting before laundering when viewed over a black backgrcund. The laundered batting shall not demonstrate a thickness reduction greater than 10 percent from its measured thic
23、kness before laundering when tested as specified in 4.4.3. 3.5 Length and put-up. For Government procurement only, unless otherwise specified (see 6.2), the batting shall be furnished in continuous lengths of 30 yards each, and shall be put-up as specified in 5.1.1. 3.6 Workmanship. The batting shal
24、l conform to the quality of product established by this specification and the occurrence of defects shall not exceed the applicable acceptable quality levei. 4. QUALITY ASSURANCE PROVISIONS 4.1 Responsibility for inspection. Unless otherwise specified in the contract or purchase order, the contracto
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- DLAMILB443461989BATTINGSYNTHETICFIBERMEDIUMDENSITY 密度 合成纤维 棉絮 PDF

链接地址:http://www.mydoc123.com/p-689553.html