1、 A-A-55217B SUPERSEDING March 29, 2011 A-A-55217A March 16, 2007 COMMERCIAL ITEM DESCRIPTION THREAD, ARAMID, SPUN STAPLE The General Services Administration has authorized the use of this commercial item description as a replacement for MIL-T-83193 for all federal agencies. 1. SCOPE. This commercial
2、 item description covers the requirements for a spun staple, Flame Resistant (FR) high temperature aramid thread. The thread is used in sewing FR protective combat apparel and FR flight safety equipment. 2. CLASSIFICATION. Type I - Normal performance. Type II - High performance. 3. SALIENT CHARACTER
3、ISTICS. 3.1 General description. The fiber used in the manufacture of the thread shall be 1.5 to 2.0 denier per filament aramid. The finished thread shall conform to the applicable requirements of Table I or II. Unless otherwise specified, the direction of the final twist shall be “Z” for all thread
4、s. Each of the individual plies of yarn shall be initially twisted with no less than the number of turns per inch to be used in the final twist, and in the opposite direction to the final twist. The thread shall have a soft finish and contain only the minimum amount of lubricant to facilitate sewing
5、. Only non-staining and non-flame propagating finishes commonly used shall be permitted as sewing finishes unless prior approval is obtained from the contracting officer. 3.2 Physical characteristics and requirements.Physical characteristics specified in Table I and II respectively, when tested in a
6、ccordance with Table III as specified. The Type I and II threads shall conform to the Comments, suggestions, or questions on this document should be addressed to: DLA Troop Support, Attn: DSCP Standardization Team, 700 Robbins Avenue, Philadelphia, PA 19111-5096. Since contact information can change
7、, you may want to verify the currency of this address information using Acquisition Streamlining and Standardization Information System (ASSIST) online database at https:/assist.daps.dla.mil. AMSC N/A FSC 8310 INCH-POUND Provided by IHSNot for ResaleNo reproduction or networking permitted without li
8、cense from IHS-,-,-A-A -55217B 2 TABLE I. Physical characteristics of Type I (normal performance) Tex 1/ Ply Length per pound (yards) Minimum Maximum Breaking strength, (lbs.), Minimum Elongation (%) Maximum 24-27 2 14,500 - 19,700 1.3 32 35-40 3 9,200 - 13,600 2.0 32 50-60 3 6,400 - 9,600 3.0 35 70
9、-80 4 4,700 - 7,100 4.5 38 90-100 4 3,600 - 5,400 5.5 38 1/ Tex size based on weight in grams/1,000 meters thread. TABLE II. Physical characteristics of Type II (high performance) Tex 1/ Ply Length per pound (yards) Minimum Maximum Breaking strength, (lbs.), Minimum Elongation (%) Maximum 21 2 21,80
10、0 - 23,400 1.5 20 27 2 16,200 18,000 2.2 20 45 2 or 3 9,200 10,200 4.0 20 60 3 7,800 8,600 5.0 20 70 3 6,200 7,000 6.0 20 90 4 4,700 5,200 8.0 20 1/ Tex size based on weight in grams/1,000 meters thread. TABLE III. Physical requirements Characteristic Requirement Test method Fiber identification See
11、 3.1 AATCC - 20 or ASTM D 276 Denier per filament See 3.1 ASTM D 1577 Melting point (Minimum) Above 500F 1/ ASTM D 7138 Turns per inch See 3.1 ASTM D 204 Twist balance See 3.1 ASTM D 204 Direction of Twist See 3.1 ASTM D 204 Tex See Tables I and II 2/ ASTM D 204 Ply See Tables I and II ASTM D 204 Le
12、ngth per pound (yards) See Tables I and II ASTM D 1907, 3/ Breaking Strength See Tables I and II Initial (Minimum) See Tables I and II ASTM D 204, 4/ After aging (Minimum) 85% of initial break strength See 3.3 ASTM D 204, 4 Elongation,% (Maximum) See Tables I and II ASTM D 204, 5/ Colorfastness (Min
13、imum) Laundering (After 3 cycles) 3-4 AATCC 61 6/, 7/, 8/, 9/ 1/ Fiber shall not carbonize at a temperature below 500F 2/ One determination per sample unit shall be made and the result reported as “pass” or “fail”. 3/ In case of dispute, a second determination (the length per pound of thread) may be
14、 determined on the thread after removal of finish. Yards/lb = weight of specimen in grams 453.6 x (number of yards in specimen) Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-A-A -55217B 3 4/ Straight strength and elongation of conditioned threads t
15、est 5/ Elongation at sewing forces test 6/ Two to six grams of the yarn, held together to form a unit for testing. Unless otherwise specified in the procurement document, the laundering cycle of the Launder-O- Meter or similar machine shall be 30 minutes and the temperature of the container and its
16、contents shall be maintained at 150 (+ 5) F. 7 The specimens must be dried after each of the three launderings 8/ AATCC Evaluation Procedure 2, Gray Scale for Staining- Only the stain on the nylon fiber of the color transfer cloth shall be evaluated for the color transfer evaluation. 9/ AATCC Evalua
17、tion Procedure 1, Gray Scale for Color Change. 3.3 Heat aging test. Five specimen skeins, of 15 yards each, shall be prepared as specified in ASTM D 1578 Option 1, using 20 turns. The five skeins shall be exposed in a hot air convection (circulating air) oven at a temperature of 550(+ 10) F for a pe
18、riod of 20 (+ 2) minutes. Upon removal, the specimens shall be conditioned at standard atmospheric conditions for 4 hours and then tested for breaking strength as specified in Table III. The heat aging resistance shall be the average of the breaking strength obtained from the specimens tested, and s
19、hall be reported to the nearest 1.0 percent of the original breaking strength. 3.4 Color. The color shall be as specified in the applicable end item specification or in the contract order. The dyed thread shall be a good match to the applicable end item when examined in accordance with 3.6. 3.5 Fini
20、sh removal procedure. Before evaluation for shade matching and testing for colorfastness or in case of dispute for Tex Size verification, except for colorfastness to wet dry cleaning, the thread shall be wet dry cleaned in accordance with AATCC-132. Excess solvent shall be removed by centrifuging or
21、 wringing. The sample shall then be rinsed in distilled water at 120 F to 160 F and dried at a temperature not exceeding 180 F. The dried sample shall then be conditioned for a minimum of 4 hours prior to evaluation for colorfastness as specified in Table III or shade matching as specified in 3.6. 3
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- DLAAA55217B2011THREADARAMIDSPUNSTAPLEPDF