SAE AMS 6365K-2014 Steel Tubing Seamless 0 95Cr - 0 20Mo (0 33 - 0 38C) (SAE 4135) Normalized or Stress Relieved (UNS G41350)《SAE 4135正火或应力消除的0 95Cr-0 20Mo (0 33-0 38C)无缝钢管件》.pdf
《SAE AMS 6365K-2014 Steel Tubing Seamless 0 95Cr - 0 20Mo (0 33 - 0 38C) (SAE 4135) Normalized or Stress Relieved (UNS G41350)《SAE 4135正火或应力消除的0 95Cr-0 20Mo (0 33-0 38C)无缝钢管件》.pdf》由会员分享,可在线阅读,更多相关《SAE AMS 6365K-2014 Steel Tubing Seamless 0 95Cr - 0 20Mo (0 33 - 0 38C) (SAE 4135) Normalized or Stress Relieved (UNS G41350)《SAE 4135正火或应力消除的0 95Cr-0 20Mo (0 33-0 38C)无缝钢管件》.pdf(6页珍藏版)》请在麦多课文档分享上搜索。
1、_SAE Technical Standards Board Rules provide that: “This report is published by SAE to advance the state of technical and engineering sciences. The use of this report is entirely voluntary, and its applicability and suitability for any particular use, including any patent infringement arising theref
2、rom, is the sole responsibility of the user.”SAE reviews each technical report at least every five years at which time it may be revised, reaffirmed, stabilized, or cancelled. SAE invites your written comments and suggestions.Copyright 2014 SAE InternationalAll rights reserved. No part of this publi
3、cation may be reproduced, stored in a retrieval system or transmitted, in any form or by any means, electronic, mechanical, photocopying, recording, or otherwise, without the prior written permission of SAE.TO PLACE A DOCUMENT ORDER: Tel: 877-606-7323 (inside USA and Canada)Tel: +1 724-776-4970 (out
4、side USA)Fax: 724-776-0790Email: CustomerServicesae.orgSAE WEB ADDRESS: http:/www.sae.orgSAE values your input. To provide feedbackon this Technical Report, please visithttp:/www.sae.org/technical/standards/AMS6365KAEROSPACE MATERIAL SPECIFICATIONAMS6365 REV. KIssued 1942-06Reaffirmed 2006-02Revised
5、 2014-07Superseding AMS6365JSteel Tubing, Seamless0.95Cr - 0.20Mo (0.33 - 0.38C) (SAE 4135)Normalized or Stress Relieved(Composition similar to UNS G41350)RATIONALEAMS6365K results from a Five Year Review and update of this specification.1. SCOPE1.1 FormThis specification covers an aircraft-quality,
6、 low-alloy steel in the form of seamless tubing.1.2 ApplicationThis tubing has been used typically for thin wall-thickness sections where minimum tensile strength up to 160 ksi (1103 MPa) is required and where parts may be welded during fabrication, but usage is not limited to such applications.2. A
7、PPLICABLE DOCUMENTSThe issue of the following documents in effect on the date of the purchase order forms a part of this specification to the extent specified herein. The supplier may work to a subsequent revision of a document unless a specific document issue is specified. When the referenced docum
8、ent has been cancelled and no superseding document has been specified, the last published issue of that document shall apply.2.1 SAE PublicationsAvailable from SAE International, 400 Commonwealth Drive, Warrendale, PA 15096-0001, Tel: 877-606-7323 (inside USA and Canada) or 724-776-4970 (outside USA
9、), www.sae.org.AMS2253 Tolerances, Carbon and Alloy Steel TubingAMS2259 Chemical Check Analysis Limits, Wrought Low-Alloy and Carbon SteelsAMS2301 Cleanliness, Aircraft Quality Steel, Magnetic Particle Inspection ProcedureAMS2370 Quality Assurance Sampling and Testing, Carbon and Low-Alloy Steel Wro
10、ught Products and Forging StockSAE INTERNATIONAL AMS6365K Page 2 of 6AMS2807 Identification, Carbon and Low-Alloy Steels, Corrosion and Heat Resistant Steels and Alloys, Sheet, Strip, Plate and Aircraft Tubing2.2 ASTM PublicationsAvailable from ASTM International, 100 Barr Harbor Drive, P.O. Box C70
11、0, West Conshohocken, PA 19428-2959,Tel: 610-832-9585, www.astm.org.ASTM A 370 Mechanical Testing of Steel ProductsASTM E 112 Determining Average Grain SizeASTM E 350 Chemical Analysis of Carbon Steel, Low-Alloy Steel, Silicon Electrical Steel, Ingot Iron, and Wrought IronASTM E 384 Knoop and Vicker
12、s Hardness of MaterialsASTM E 1444 Magnetic Particle Testing3. TECHNICAL REQUIREMENTS3.1 CompositionShall conform to the percentages by weight shown in Table 1, determined by wet chemical methods in accordance with ASTM E 350, by spectrochemical methods, or by other analytical methods acceptable to
13、purchaser:TABLE 1 - COMPOSITIONElement min maxCarbon 0.33 0.38Manganese 0.70 0.90Silicon 0.15 0.35Phosphorus - 0.025Sulfur - 0.025Chromium 0.80 1.10Molybdenum 0.15 0.25Nickel - 0.25Copper - 0.353.1.1 Check AnalysisComposition variations shall meet the applicable requirements of AMS2259.3.2 Condition
14、Cold finished and either normalized and tempered, stress relieved, or otherwise heat treated.3.3 PropertiesTubing shall conform to the following requirements; hardness and tensile testing shall be performed in accordance with ASTM A 370:3.3.1 Tensile PropertiesShall be as shown in Table 2.SAE INTERN
15、ATIONAL AMS6365K Page 3 of 6TABLE 2A - MINIMUM MECHANICAL PROPERTIES, INCH/POUND UNITSNominal ODInchNominal WallThicknessInchTensileStrengthksiYield Strengthat 0.2% OffsetksiElongation in2 Inches%Full TubeElongation in2 Inches%StripUp to 0.500, excl Up to 0.188, incl 100 85 8 -Up to 0.500, excl Over
16、 0.188 95 80 10 -0.500 and over Up to 0.188, incl 100 85 12 70.500 and over Over 0.188 95 80 15 10TABLE 2B - MINIMUM MECHANICAL PROPERTIES, SI UNITSNominal ODMillimetersNominal WallThicknessMillimetersTensileStrengthMPaYield Strengthat 0.2% OffsetMPaElongation in50.8 mm%Full TubeElongation in50.8 mm
17、%StripUp to 12.70, excl Up to 4.78, incl 689 586 8 -Up to 12.70, excl Over 4.78 655 552 10 -12.70 and over Up to 4.78, incl 689 586 12 712.70 and over Over 4.78 655 552 15 103.3.2 Average Grain SizeShall be ASTM No. 5 or finer, determined in accordance with ASTM E 112.3.3.3 Decarburization3.3.3.1 Tu
18、bing ordered ground, turned, or polished shall be free from decarburization on the ground, turned, or polished surfaces. Decarburization on tubing ID shall not exceed the maximum depth specified in Table 3.3.3.3.2 Allowable decarburization of pierced billets, of tubing for redrawing, or of tubing or
19、dered to specified microstructural requirements shall be as agreed upon by purchaser and vendor.3.3.3.3 Tubing to which 3.3.3.1 or 3.3.3.2 is not applicable shall be free from complete decarburization. Partial decarburization shall not exceed the limits shown in Table 3.TABLE 3A - MAXIMUM DECARBURIZ
20、ATION LIMITS, INCH/POUND UNITSNominal Wall Thicness (T)InchDepth of Partial DecarburizationInchIDDepth of Partial DecarburizationInchODDepth of Partial DecarburizationInchID+ODUp to 0.040, incl 0.18T 0.18T 0.25TOver 0.040 to 0.050, incl 0.009 0.009 0.012Over 0.050 to 0.070, incl 0.010 0.010 0.014Ove
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- SAEAMS6365K2014STEELTUBINGSEAMLESS095CR020MO033038CSAE4135NORMALIZEDORSTRESSRELIEVEDUNSG41350SAE4135

链接地址:http://www.mydoc123.com/p-1022386.html