《SAE AMS 4520L-2015 Leaded Phosphor Bronze Strip 88 5Cu - 4 0Sn - 4 0Pb - 3 0Zn - 0 26P Cold Rolled Half Hard (HO2) (UNS C54400).pdf》由会员分享,可在线阅读,更多相关《SAE AMS 4520L-2015 Leaded Phosphor Bronze Strip 88 5Cu - 4 0Sn - 4 0Pb - 3 0Zn - 0 26P Cold Rolled Half Hard (HO2) (UNS C54400).pdf(5页珍藏版)》请在麦多课文档分享上搜索。
1、AEROSPACE MATERIAL SPECIFICATION AMS4520 REV. L Issued 1940-01 Revised 2015-01 Superseding AMS4520K Leaded Phosphor Bronze Strip 88.5Cu - 4.0Sn - 4.0Pb - 3.0Zn - 0.26P Cold Rolled, Half Hard (HO2) (Composition similar to UNS C54400) RATIONALE AMS4520L revises Composition (Table 1, 3.1.2) and is a Fi
2、ve Year Review and update of this specification. 1. SCOPE 1.1 Form This specification covers a copper alloy in the form of strip. 1.2 Application This strip has been used typically for rolled, split bushings, but usage is not limited to such applications. 2. APPLICABLE DOCUMENTS The issue of the fol
3、lowing documents in effect on the date of the purchase order forms a part of this specification to the extent specified herein. The supplier may work to a subsequent revision of a document unless a specific document issue is specified. When the referenced document has been cancelled and no supersedi
4、ng document has been specified, the last published issue of that document shall apply. 2.1 SAE Publications Available from SAE International, 400 Commonwealth Drive, Warrendale, PA 15096-0001, Tel: 877-606-7323 (inside USA and Canada) or 724-776-4970 (outside USA, www.sae.org. AMS2222 Tolerances, Co
5、pper and Copper Alloy Sheet, Strip, and Plate _ SAE Technical Standards Board Rules provide that: “This report is published by SAE to advance the state of technical and engineering sciences. The use of this report is entirely voluntary, and its applicability and suitability for any particular use, i
6、ncluding any patent infringement arising therefrom, is the sole responsibility of the user.” SAE reviews each technical report at least every five years at which time it may be revised, reaffirmed, stabilized, or cancelled. SAE invites your written comments and suggestions. Copyright 2015 SAE Intern
7、ational All rights reserved. No part of this publication may be reproduced, stored in a retrieval system or transmitted, in any form or by any means, electronic, mechanical, photocopying, recording, or otherwise, without the prior written permission of SAE. TO PLACE A DOCUMENT ORDER: Tel: 877-606-73
8、23 (inside USA and Canada) Tel: +1 724-776-4970 (outside USA) Fax: 724-776-0790 Email: CustomerServicesae.org SAE WEB ADDRESS: http:/www.sae.org SAE values your input. To provide feedback on this Technical Report, please visit http:/www.sae.org/technical/standards/AMS4520L SAE INTERNATIONAL AMS4520L
9、 Page 2 of 5 2.2 ASTM Publications Available from ASTM International, 100 Barr Harbor Drive, P.O. Box C700, West Conshohocken, PA 19428-2959, Tel: 610-832-9585, www.astm.org. ASTM B248 General Requirements for Wrought Copper and CopperAlloy Plate, Sheet, Strip, and Rolled Bar ASTM B248M General Requ
10、irements for Wrought Copper and CopperAlloy Plate, Sheet, Strip, and Rolled Bar (Metric) ASTM E8/E8M Tension Testing of Metallic Materials ASTM E478 Chemical Analysis of Copper Alloys 3. TECHNICAL REQUIREMENTS 3.1 Composition Shall conform to the percentages by weight shown in Table 1, determined by
11、 wet chemical methods in accordance with ASTM E478, by spectrochemical methods, or by other analytical methods acceptable to purchaser. Table 1 - Composition Element min max Tin 3.5 4.5 Lead 3.0 4.0 Zinc 1.5 4.5 Phosphorus 0.01 0.50 Iron - 0.10 Copper (3.1.2) remainder - Sum of Named Elements (3.1.3
12、) 99.5 - 3.1.1 These composition limits do not preclude the presence of other elements. Limits may be established and analysis required for unnamed elements by agreement between the manufacturer or supplier and purchaser. 3.1.2 Copper may be reported as “remainder”, or as the difference between the
13、sum of results for all analyzed elements and 100%, or as the result of direct analysis. 3.1.3 When all the elements in the table are analyzed, the sum shall be 99.5% minimum, but such determination is not required for routine acceptance of each lot. 3.2 Condition Cold rolled, half hard (H02) temper
14、(See 8.3). 3.3 Properties Strip shall conform to the following requirements: 3.3.1 Tensile Strength, Ultimate Shall be 55.0 to 70.0 ksi (379 to 483 MPa). 3.3.2 Elongation Shall not be lower than 16% in 2 inches (50.8 mm), determined in accordance with ASTM E8/E8M. SAE INTERNATIONAL AMS4520L Page 3 o
15、f 5 3.4 Quality Strip, as received by purchaser, shall be uniform in quality and condition, sound, and free from foreign materials and from imperfections detrimental to usage of the strip. 3.5 Tolerances Shall conform to AMS2222 as applicable to nonrefractory alloys. 4. QUALITY ASSURANCE PROVISIONS
16、4.1 Responsibility for Inspection The vendor of strip shall supply all samples for vendors tests and shall be responsible for the performance of all required tests. Purchaser reserves the right to sample and to perform any confirmatory testing deemed necessary to ensure that the strip conforms to sp
- 1.请仔细阅读文档,确保文档完整性,对于不预览、不比对内容而直接下载带来的问题本站不予受理。
- 2.下载的文档,不会出现我们的网址水印。
- 3、该文档所得收入(下载+内容+预览)归上传者、原创作者;如果您是本文档原作者,请点此认领!既往收益都归您。
下载文档到电脑,查找使用更方便
10000 积分 0人已下载
下载 | 加入VIP,交流精品资源 |
- 配套讲稿:
如PPT文件的首页显示word图标,表示该PPT已包含配套word讲稿。双击word图标可打开word文档。
- 特殊限制:
部分文档作品中含有的国旗、国徽等图片,仅作为作品整体效果示例展示,禁止商用。设计者仅对作品中独创性部分享有著作权。
- 关 键 词:
- SAEAMS4520L2015LEADEDPHOSPHORBRONZESTRIP885CU40SN40PB30ZN026PCOLDROLLEDHALFHARDHO2UNSC54400PDF

链接地址:http://www.mydoc123.com/p-1021671.html