    NASA-TN-D-2331-1964 Fatigue-crack propagation in several titanium and stainless-steel alloys and one superalloy《在若干钛和不锈钢合金及一个超耐热不锈钢上的疲劳裂缝扩展》.pdf

    • 资源ID:836795       资源大小:542.52KB        全文页数:33页
    • 资源格式: PDF        下载积分:10000积分
    快捷下载 游客一键下载
    账号登录下载
    微信登录下载
    二维码
    微信扫一扫登录
    下载资源需要10000积分(如需开发票,请勿充值!)
    邮箱/手机:
    温馨提示:
    如需开发票,请勿充值!快捷下载时,用户名和密码都是您填写的邮箱或者手机号,方便查询和重复下载(系统自动生成)。
    如需开发票,请勿充值!如填写123,账号就是123,密码也是123。
    支付方式: 支付宝扫码支付    微信扫码支付   
    验证码:   换一换

    加入VIP,交流精品资源
     
    账号:
    密码:
    验证码:   换一换
      忘记密码?
        
    友情提示
    2、PDF文件下载后,可能会被浏览器默认打开,此种情况可以点击浏览器菜单,保存网页到桌面,就可以正常下载了。
    3、本站不支持迅雷下载,请使用电脑自带的IE浏览器,或者360浏览器、谷歌浏览器下载即可。
    4、本站资源下载后的文档和图纸-无水印,预览文档经过压缩,下载后原文更清晰。
    5、试题试卷类文档,如果标题没有明确说明有答案则都视为没有答案,请知晓。

    NASA-TN-D-2331-1964 Fatigue-crack propagation in several titanium and stainless-steel alloys and one superalloy《在若干钛和不锈钢合金及一个超耐热不锈钢上的疲劳裂缝扩展》.pdf

    1、NASA TECHNICAL NOTE v cr) cr) N ti z c NASA TN D-2331 - FATIGUE-CRACK PROPAGATION IN SEVERAL TITANIUM AND AND ONE SUPERALLOY STAINLESS-STEEL ALLOYS Langley Research Center Langley Station, Hampton, Va. + NATIONAL AERONAUTICS AND SPACE ADMINISTRATION WASHINGTON, D. C. OCTOBER 1964 5 Provided by IHSNo

    2、t for ResaleNo reproduction or networking permitted without license from IHS-,-,-1 TECH LIBRARY KAFB, NM I Illill Ill11 111ll lllll I1ll1 Mll11111111 0077545 FATIGUE-CRACK PROPAGATION IN SEVERAL TITANIUM AND STAINLESS-STEEL ALLOYS AND ONE SUPERALLOY By C. Michael Hudson Langley Research Center Langl

    3、ey Station, Hampton, Va. NATIONAL AERONAUTICS AND SPACE ADMINISTRATION _ For sale by the Office of Technical Services, Deportment of Commerce, Woshington, D.C. 20230 - Price $0.75 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-FATIGUE-CRACK PROPAGAT

    4、ION IN SENERAL TITANIUM AND STAINLESS-STEEL ALLOYS AND ONE SUPERALLOY By C. Michael Hudson SUMMARY Axial-load fatigue-crack-propagation tests were conducted on 8-inch-wide (20.3-cm) sheet specimens made of Ti-4Al-Po-lV (Aged), Ti-6U-4V (Annealed) , and Ti-8Al-lMo-lV (Triplex Annealed) titanium alloy

    5、s, AM 350 (20-percent CRT) , AM 350 (Double Aged), PH 14-8Mo (SRH 950), PH 15-7Mo (TH 1050), and AIS1 301 (50-percent CR) stainless steels, and Rene 41 (Condition B). Tests were run at 800 F (300 K), 50 F (5610 K), and, in some cases, -logo F (195O K) to deter- mine the effect of temperature on the

    6、fatigue-crack-propagation characteristics a of each material. The materials are ranked according to their resistance to fatigue-crack propagation, and Ti-8Al-lMo-lV (Triplex Annealed) appeared to be the most resist- ant over the temperature range of the investigation. Special apparatus developed for

    7、 the elevated- and cryogenic-temperature studies are described herein. INTRODUCTION The elevated temperatures associated with aircraft flying at a Mach number of approximately 2.5 and faster precludes the use of aluminum alloys for struc- tural components. Consequently, aircraft designers must turn

    8、to more heat- resistant materials with which they have had little aircraft-design experience. Important to the selection of these materials is their resistance to fatigue- crack propagation and the effect of temperature on this resistance. Designers know that fatigue cracks will probably form in the

    9、ir aircraft structures, and consequently they must select materials having high resistance to crack growth in order to minimize the danger of fatigue failure. An investigation has been undertaken to evaluate the crack-propagation char- acteristics of nine materials suitable for use at elevated tempe

    10、ratures. This investigation included tests of the nine materials at room temperature of 80 F (300 K) and at elevated temperature of 550 (SIo K) . the effects of temperature on fatigue-crack growth, two of the materials were To evaluate further Provided by IHSNot for ResaleNo reproduction or networki

    11、ng permitted without license from IHS-,-,-tested at the cryogenic temperature of -109 F (195 K). ducted at positive mean stresses on sheet specimens made of five stainless steels, three titanium alloys, and one superalloy. Tests have been con- The present paper presents the experimental results of t

    12、his study. Included are effects of temperature on crack propagation in each material and a relative ranking of each material with respect to resistance to crack growth at each test temperature. All physical properties in this paper are given in both U.S. Customary Units and the International System

    13、of Units. An appendix is included to explain the relationship between the two systems. E Youngs modulus, ksi or giganewtons/meter2 ( GN/m2) e total elongation in 2-inch- (3.08-cm) gage length, percent N number of cycles R ratio of minimum stress to maximum stress Sa s, 0, aY X one-half of total leng

    14、th of central symmetrical crack, inches or alternating stress amplitude, ksi or meganewtons/meter2 ( MN/m2 ) mean stress, ksi or meganewtons/meter* (MI?/m2) ultimate tensile strength, ksi or meganewtons/meter2 ( MN/m2) yield strength (0.2-percent off set), ksi or meganewtons/meter2 (MN/m2) centimete

    15、rs (cm) SPECIMENS AND TESTS Specimens The five stainless steels, three titanium alloys, and one superalloy studied in this investigation are listed as follows: AIS1 301 (50-percent Cold Rolled - eR) AM 350 (20-percent Cold Rolled and Tempered - CRT) AM 350 (Double Aged - DA) PH 15-“0 (TH 1050) 2 Pro

    16、vided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-PH 14-8Mo (SFB 950) Re consequently, the cutting proc- ess was believed to have little effect upon the material surrounding the notch. The heat gener- A reference grid (fig. 2) was photographically printed

    17、 on the surface of the specimen to mark intervals in the path of the crack. This reference grid Figure 2.- Grid used to mark intervals in crack path. 6 Notch LCen t ral L-63-4299.1 Grid spacing is 0.05 in. (1.27 mm). afforded ready observation of the crack front and provided a crack-growth path free

    18、 of mechanical defects which might affect normal crack propagation. adopting the photographic reference grid, it was determined by metallographic examinations and tensile tests on specimens bearing the grid that the grid had no detrimental effects upon the materials at 550 F (561O K). Before Testing

    19、 Equipment Axial-load fatigue-testing equipment used in this investigation included a subresonant machine, a hydraulic machine, and a combination hydraulic and sub- resonant machine. The subresonant machine had an operating frequency of 1800 cpm, a load capacity of ?20,000 pounds (+89 m), and cycle-

    20、counter reading in units of 100 clycles. The hydraulic machine had an operating frequency of Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-1200 cpm, a load capacity of 100,000 pounds (445 kN), and a cycle-counter reading in units of 100 cycles. As

    21、a hydraulic unit, the combination machine had an operating frequency of 50 cpm, a load capacity of 132,000 pounds (587 kN), and a cycle-counter reading in units of 1 cycle. As a subresonant unit this machine had an operating frequency of 820 cpm for the specimens used (a func- tion of the natural fr

    22、equency of the system), a load capacity of 110,000 pounds (489 kN), and a counter reading in units of 100 cycles. machines is further described in references 1, 2, and 3, respectively. Each of these testing Loads were monitored continuously by measuring the output of a strain-gage bridge cemented to

    23、 a weigh bar in series with the specimen. sion was approximately k1 percent. Heat-deflecting baffles were used for ther- mal protection of the weigh bars on the 20,000-pound (89-k) and the 100,000- pound (445-kN) testing machines. In the combination testing machine, no thermal protection was require

    24、d for the weigh bars because of the horizontal arrangement of the bar with respect to the heating furnace. Monitoring preci- Special apparatus was developed to conduct the elevated-temperature tests (fig. 3). Three 1/2-inch-thick (l.27-cm) graphite blocks were placed in contact 7 Carbon Block -Heati

    25、ng Slab Pressure Plote Pressure Screw Steel Fromework -Viewing Slot -Specimen Location L-65-9528.1 Figure 3.- Elevated-temperature-test apparatus. with the specimens. Go were placed on the observation side, one above and the other below the region of crack growth. A 1/2-inch (1.27-cm) gap was used t

    26、o provide an unobstructed view of the growing crack. The third block was located on the opposite surface of the specimen immediately adjacent to the crack-growth region. Adjacent to each graphite block was a ceramic heating slab and an insulating pressure plate, in that order. A steel framework havi

    27、ng an observation cutout was used to hold the components in position during testing. The components were held against the specimen by three machine screws which jammed against the asbes- tos pressure plate. The screws were carefully tightened to insure thermal contact without introducing significant

    28、 friction forces. The surfaces of each component were machine ground until 90-percent contact was obtained between the surfaces of adjacent components and between the graphite and the specimens. A chromel-alumel control thermo- couple was spot welded in the pro- jected crack path near the edge of th

    29、e specimen. In preliminary tests, the temperature variation across the width of the specimen using an edge control point was found to be less than k5O F (k3O K). 5 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-Temperature control was maintained wit

    30、hin f2O F (+lo K) in the 550 F (561O K) tests by a controller recorder which regulated current through a satu- rable reactor. The 60-cycle single-phase a-c controller operated on 208 volts. The equipment used to conduct the cryogenic-temperature tests is shown in figure 4. Solid blocks of dry ice we

    31、re mounted in the same steel framework used .- Pressure Plate -Pressure Screw Steel Framework -Viewing Slot - L-65-9529 .1 L-63-9530 (a) Steelwork with dry ice installed. (b) Insulating box installed. Figure 4.- Cryogenic-temperature-test apparatus. for the furnace. surface in the same manner as the

    32、 heating components. The temperature was con- trolled by the temperature of the dryice and was found to vary less than +2O F (+lo K) across the width of the specimen. The average temperature was found to vary less than +5O F (*3O K) during the course of a test. The sublimation rate of the dry ice wa

    33、s satisfactorily controlled by insulating the entire cooling 6 These dry-ice blocks were held directly against the specimen Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-apparatus from circulating air drafts. Frost buildup on the specimen surface w

    34、as controlled by periodically spraying the specimen with ethyl alcohol. In all the room-temperature tests and in the elevated- and cryogenic- temperature tests in which compressive loadings were applied, two lubricated guides similar to those described in reference 4 were used to prevent buckling an

    35、d out-of-plane vibrations. Light oil was used to lubricate the surfaces of the specimen and of the guides in the room-temperature and cryogenic-temperature tests. In the elevated-temperature tests dry molybdenum disulfide was used for the lubricant. One of the two plates contained a 1/2-inch-wide (1

    36、.27-ma) cutout across the width of the plate to allow visual observation of the region of the crack. In the room- and cryogenic-temperature tests, a clear Plexiglas insert was fitted into the cutout to prevent buckling in the observation region. In the elevated-temperature tests, a pyrex insert was

    37、used for this purpose. Test Procedure Constant-amplitude axial-load fatigue tests were conducted under positive mean stresses of 40 ksi (276 MN/m*) for the stainless steels and Re 41 was slightly lower at elevated temperature than at room temperature. The crack-propagation curves for AISI 3Ol and AM

    38、 350 (20-percent CRT) in of 20 ksi (138 MN/m2) and higher, the figures 5 and 6 indicate that, for cracks grew much faster at elevated temperature than at room temperature. For Sa slightly faster at room temperature than at elevated temperature. No explana- tion for this small reversal in resistance

    39、to crack growth can currently be offered. The decreased resistance at elevated temperature at the higher stress levels may be attributed to the deterioration of tensile properties at that temperature. Sa of 10 ksi (68 MN/m2) and 5 ksi (34 MN/m2) cracks in these two materials grew The crack-propagati

    40、on curves for AM 350 (DA), PH 15-Mo, FH 14-8M0, and Re + c m - aJ 0.5 1 0 0 L 0 0 - - Sa = 20 ksi ( I38 MN/m21 Sa = 5 ksi (35 MN/m21 - 8OoF ( 300K) 55O0F(56l0K1 -I 80F ( 300K I _ -2.5 2.0 -I .5 .o 0.5 0 81 11 I 101 I 03 I 05 I 07 N. cycles ,I 101 i2e5 Sa = 40 ksi (276 MN/m21 S50F( 56 I OK1 - Sa = IO

    41、 ksi (69 MN/m2) 12.5 I I N. cvcles N. cvcles ; IT w C aJ m - Y 0 0 L 0 Figure 5.- Fatigue crack-propagation curves for AIS1 301 (50-percent CR). S, = 40 ksi (276 MN/m2). 9 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-I .o C ._ S +. m 5 0.5 - Y 0 0

    42、 L 0 0 I .o C ._ C +. m c _“ 0.5 Y 0 0 L 0 0 Sa = 60 ksi (414 MN/m2) sa = 20 ksi (138 MN/m2) I I ,I-,I 81 1 +. IJI - Y 0 0 0.5 2.5 2.0 ; 0 S +. 1.5 W - Y .o 0 L 0 0.5 0 2.5. 2.0 . E 0 .c m C W I .5 - - 1.0 Y 0 L 0 D.5 n 0 I 101 I 03 I 05 I 07 N. cvcles Figure 6.- Fatigue crack-propagation curves for

    43、 AM 350 (20-percent CRT). S, = 40 ksi (276 MN/m2). 10 .- . . . -I Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-I .o - - 60F(300K) 550F( 56 I OK) c ._ 2.0 ; 1.5 c- + m c D -1.0 - 1 0 0 L -0.5 “ m 6 0.5 - Y 0 0 L 0 C + c m - - 0.5 1 “ L 0 0 0 Sa = 6

    44、0 ksl (414 MN/m21 I I I I I I .o C C + C m - 0.5 1 “ L 0 0 L 1 L Sa = 20 ksi ( 138 MN/mz) 1 L S, = 40 ksi (276 MN/m2) ,I I1 I I 1 I 1 I 101 I 03 I 05 I 07 N. cycles -I 2.0 ; q I I I I I I lo I 1 2.5 Sa = 10 ksi (69 MN/m2) 80F( 550aF( II II L N. cycles Sa = 5 ksi (35 MN/m2) I 101 I 03 N. 72.5 - 2.0 0

    45、 0.5 I 07 ,I I I 05 cvcles Figure 7.- Fatigue crack-propagation curves for AM 350 (DA). S, = 40 ksi (276 MN/m2). 11 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-I .0 C ._ S + m k 0.5 - Y 0 0 L 0 c .c c + m 0 0 L “ Y 0 I .o .- - 0 0.5 Sa = 60 ksi (

    46、414 MN/vJ r - Sa = IO ksi (59 MN/m2) -2.5 - 2 .0 - 1.c 0 - 0.5 I ,I ,I ,I ti IO - S, = 20 ksi (138 MN/m2) 80F(3000K1 55OoF ( 56 I OK) - I L_LIl L S5OoF (56 I OK). - - 0 So = 40 ksi (276 MN/m21 -2.5 -2.0 -I .5 I .0 0.5 2.5 2.0 . E 1.5 C 0 - 1.0 Y 0 L 0 1.5 0 0 I ,I ,I ,I ,I 11 N. cycles 0 S * m c 0 -

    47、 Y o L 0 Figure 8.- Fatigue crack-propagation curves for PH 15-7Mo (TR 1050). S, = 40 ksi (276 MN/m2). 12 Provided by IHSNot for ResaleNo reproduction or networking permitted without license from IHS-,-,-I .o c ._ C + m c - 0 0.5 1 0 0 L 0 0 I .o C + m c w 0.5 0 1 0 L U 0 1 Sa = 60 ksi I414 MN/m2) -

    48、 Sa = 20 ksi 138 MN/) -105F( 195:K) - ttOF(300 Kl 55OOF ( 56 I K 1 101 I 03 I 05 107 , 101 I 03 I 05 I 07 1 2.5 Sa = 40 ksi (276 MN/m2) -109F( 195K) 8OoF( 300K) 550F(56loKl -. 3 C BOF( 300K) - Oe5 * 55O0F(56l0K) 550F ( 56 I OK I -1.0 0 0 L 1 0 0 0.5 ._ r + m I .O r Sa = IO ksi (69 MN/m21 - C ._ + r m 0 0.5 - - 55OoF( 56 IK) C 80F( 300K) - - Y 0 L 0 0 I I I I I I - sa = 5 ksi (35 MN/mz) -2.5 -2.0 ; 0 r w -1.5 al 550F( 80F( 300KI 56 IKI - Y -1.0 g L 0 -0.5 I ,I I 1 I I 0 N. cycles N. cycles E 0 Y 0 0 L u I 101 I 03


    注意事项

    本文(NASA-TN-D-2331-1964 Fatigue-crack propagation in several titanium and stainless-steel alloys and one superalloy《在若干钛和不锈钢合金及一个超耐热不锈钢上的疲劳裂缝扩展》.pdf)为本站会员(李朗)主动上传,麦多课文档分享仅提供信息存储空间,仅对用户上传内容的表现方式做保护处理,对上载内容本身不做任何修改或编辑。 若此文所含内容侵犯了您的版权或隐私,请立即通知麦多课文档分享(点击联系客服),我们立即给予删除!




    关于我们 - 网站声明 - 网站地图 - 资源地图 - 友情链接 - 网站客服 - 联系我们

    copyright@ 2008-2019 麦多课文库(www.mydoc123.com)网站版权所有
    备案/许可证编号:苏ICP备17064731号-1 

    收起
    展开